WO2014084828A1 - Alkenyl succinic acids or anhydrides as corrosion inhibitors for metal surfaces - Google Patents

Alkenyl succinic acids or anhydrides as corrosion inhibitors for metal surfaces Download PDF

Info

Publication number
WO2014084828A1
WO2014084828A1 PCT/US2012/067011 US2012067011W WO2014084828A1 WO 2014084828 A1 WO2014084828 A1 WO 2014084828A1 US 2012067011 W US2012067011 W US 2012067011W WO 2014084828 A1 WO2014084828 A1 WO 2014084828A1
Authority
WO
WIPO (PCT)
Prior art keywords
benzene
recited
asa
acidic medium
corrosive
Prior art date
Application number
PCT/US2012/067011
Other languages
French (fr)
Inventor
John Link
Original Assignee
General Electric Company
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by General Electric Company filed Critical General Electric Company
Priority to CN201280077405.4A priority Critical patent/CN104812942A/en
Priority to PCT/US2012/067011 priority patent/WO2014084828A1/en
Priority to EP12799018.2A priority patent/EP2925907B1/en
Priority to US14/443,733 priority patent/US9732429B2/en
Publication of WO2014084828A1 publication Critical patent/WO2014084828A1/en

Abstract

Methods of inhibiting corrosion in a benzene distillation or dryer unit are provided wherein alkenyl succinic acids or anhydrides (ASA) are brought into contact with metal surfaces thereby protecting the metal from an acidic corrosive medium flowing through the overhead. The benzene distillation column or drying tower may be utilized to purify benzene for subsequent feed of the purified benzene to an alkylation process such as in the alkylation of benzene by ethene to form ethylbenzene utilizing a zeolite alkylation catalyst.

Description

ALKENYL SUCCINIC ACIDS OR ANHYDRIDES AS CORROSION
INHIBITORS FOR METAL SURFACES
FIELD OF INVENTION
[0001] The invention pertains to methods of inhibiting corrosion in benzene drying towers and chemical process reactors by feeding alkenylsuccinic acids or anhydrides (ASA) to contact the corrosive media contained in the tower or reactor.
BACKGROUND OF THE INVENTION
[0002] Benzene drying columns or towers are commonly employed to purify benzene for use in processes such as the alkylation of benzene to ethylbenzene (EB). In some cases, the benzene supply contains chloride salts and organic chlorine compounds. The chloride salts hydrolyze in the direct fired heater or reboiler of the tower in the presence of water. The organo chlorine compounds can undergo nucleophilic substitution, in the presence of water, to form an alcohol and HC1. The HC1 and water then travel to the overhead due to their boiling points. If untreated, the overhead lines from such benzene columns or towers are highly corrosive resulting in damage to the overhead conduits, and to condensers, heat exchangers, pumps, accumulators and the like that are in fluid communication with such conduits.
[0003] Typically, corrosion inhibitors that may be employed are amines or amine based to neutralize the corrosive acidic species. The amine based filming corrosion inhibitors form a protective barrier on the metal surfaces of the tower and ancillary equipment. Unfortunately, these nitrogen containing products poison zeolite catalysts that are often employed in the benzene alkylation processes. The present invention is directed toward the provision of effective corrosion inhibition with a non-nitrogen containing inhibitor that will not adversely affect zeolite catalysts functioning in downstream processes such as the alkylation of benzene with ethylene to form EB. The production of EB is commercially important as it is a precursor for styrene monomer. SUMMARY OF THE INVENTION
[0004] In one exemplary aspect of the invention, a method is provided for inhibiting corrosion of metal surfaces in contact with an acidic corrosive medium. An effective amount of an alkenylsuccinic acid or anhydride (both acid and anhydride form being referred to herein as "ASA") is added to the corrosive acidic medium. In certain embodiments, from about 1-500 ppm of the ASA is added to the corrosive acidic medium based upon 1 million parts of that medium. In further aspects of the invention, the ASA is devoid of nitrogen.
[0005] Generally, the ASAs are reaction products of C8-C32 olefins or mixtures thereof with maleic acid or anhydride. In certain preferred embodiments of the invention, the olefin may be a C12, C16, C18 olefin or mixtures thereof.
[0006] The acidic corrosive medium may comprise the benzene stream in the overhead section of a benzene drying column or the like. Typically, the corrosive acidic medium comprises predominantly gaseous benzene with low levels of water vapor and corrosive species such as HC1 contained therein. Commonly these media have an acidic pH of about 1-7, and in some instances, these corrosive media have a highly acidic pH range of about 2 or less.
[0007] The benzene drying tower may be adapted to purify benzene for subsequent feed of the purified benzene to a downstream chemical process such as a benzene alkylation reactor for formation of ethylbenzene (EB) from the purified benzene reactant and an ethylene reactant. In these reaction schemes, the reactants are brought into contact with a zeolite catalyst.
[0008] The invention will be described further in conjunction with the appended, illustrative drawing.
BRIEF DESCRIPTION OF THE DRAWING
[0009] Fig. 1 is a schematic diagram of a benzene drying and light end removal tower in which the corrosion inhibiting treatment of the invention may be employed. DETAILED DESCRIPTION
[0010] In one exemplary embodiment of the invention, ASA are employed as corrosion inhibitors in benzene drying columns and the like wherein benzene is processed for purification and subsequent feed to a variety of processes. In one aspect, the purified benzene is fed to a reactor along with ethene, i.e., ethylene, for alkylation of benzene to ethyl benzene. These benzene alkylation processes may be performed in either the liquid or vapor phase and the reaction is usually aided by a catalyst, such as a zeolite catalyst. Since a portion of the corrosion inhibitor persists with the benzene fed to the process, the potential for catalyst poisoning increases. This poisoning problem is especially acute when nitrogen containing corrosion inhibitors or filming amines are used in the benzene drying tower. The ASAs used in accordance with the invention are nitrogen free, provide improved corrosion inhibition results, and do not poison the zeolite catalysts that are often employed in benzene alkylation processes and the like.
[0011] As to the ASA compounds that may be used as the corrosion inhibitors, these are typically prepared by an ene reaction involving heating a C8-C32 olefin or a mixture thereof with maleic anhydride. The mole ratio of olefin to maleic anhydride may be varied but typically is within the range of about 1: 1 - 2:1. The reagents are heated and stirred at temperatures of about 180 °C - 230 °C for several hours in an inert atmosphere. Details of the synthesis of the ASAs may be gleaned by review of U.S. Patent 7,455,751 (Ward et al.) and U.S. Patent 6,867,171 (Harrison et al.), both of which are incorporated by reference herein.
[0012] The anhydride forms of the ASA may be used, but in order to be effective, these should hydrolyze to the acid form. Such hydrolysis would normally occur in the overhead. The acid form of the ASA is preferred and is prepared via reaction of the olefin with an unsaturated acidic reagent. (See U.S. Patent 6,867,171.) One of the unsaturated acidic reagents listed in the '171 patent is maleic acid or its anhydride. In addition to the unsaturated acidic reagents, a strong acid catalyst having a pKa of less than about 4 may also be employed in the reaction to form the acid form ASA. [0013] Turning now to Fig. 1, there is shown a benzene dryer and light ends removal tower 2 of the type that may be used to provide and/or recycle benzene to a benzene alkylation reactor. As shown, benzene is fed to the tower through conduit 4. This feed may for example comprise a combined feed of recycled benzene with a fresh benzene supply from a commercial supplier. In many cases, when the benzene is supplied, it may be contaminated with ionic and covalent CI. The tower 2 acts primarily as a straightforward distillation tower wherein water vapor, light hydrocarbons, and benzene are removed in the overhead lines 6 and report to condenser 8 which forwards condensed benzene to the accumulator 12 then through pump 14 and line 16 so that the benzene is fed as reflux into the tower. Acidic water is removed from the accumulator via water draw off 40. In addition to the presence of benzene and water vapor, acidic corrosive species such as HC1 are also present in the overhead line 6. Purified benzene exits as bottoms at 18 and is forwarded to the desired process such as a benzene alkylation process as shown at 20.
[0014] Advantageously, the ASA corrosion inhibitor is fed to the overhead lines as shown at 10 upstream from the condenser. The corrosion inhibitor may be fed at from about 1-500 ppm, preferably 10-80 ppm, most preferably about 50 ppm of the corrosion inhibitor based upon 1 million parts of the mixed vapor/liquid phase present in the overhead. The corrosion inhibitor can also be fed to the reflux line 16.
[0015] In one aspect of the invention, the purified benzene exiting the tower at 18 is used as a feed to either a liquid or vapor phase benzene alkylation process. Commercial ethylbenzene (EB) is produced in these processes by zeolite or other catalysis systems. The zeolite systems are becoming more prevalent, and in these systems, the catalyst may be employed in both the alkylation and transalkylation reactors. Zeolite catalysts that are commonly used include acidic zeolite / alumina and y-zeolite / alumina and other zeolite based catalysts such as dealuminized mordenite, alumina / magnesium silicate, and zeolite beta / alumina.
[0016] Generally, the corrosion inhibition methods may be used in conjunction with a variety of processes in which benzene is purified or dried in a drying or distillation column with the so-purified benzene then fed to a reactor or the like in which a zeolite catalyst will be employed to contact the reactants. For example, in addition to feed of the purified benzene to a reactor for alkylation of benzene with ethene to form ethylbenzene, the corrosion inhibition method may be used in a benzene drying or distillation column adapted to feed benzene to a reactor in which a zeolite catalyst will be employed to alkylate benzene with propylene to form cumene.
[0017] The invention will now be described in conjunction with the following illustrative examples.
EXAMPLES
[0018] In order to demonstrate the corrosion inhibitor efficacy of the ASA reaction products, modified spindle tests were undertaken. The test medium consisted of 99% toluene and 1% distilled water. The pH of the distilled water was adjusted to 2.0 with HC1. The liquid was purged with N2 and maintained at 80 °C. The spindles were immersed in the liquid medium for 1 hour and rotated therein at 300 rpm. Corrosion rate of the spindles were determined and are shown in Table I.
Table I
Corrosion inhibitor (ppm) Corrosion Rate (mpy)
C-l 16 ppm 25
C-l 8 ppm 45
Ex-1 8 ppm 25
Ex-1 16 ppm 8
C-l crude tall oil dimer and trimer acids C36-C54
Ex-1 alkenyl succinic acid C12
Field Trial
[0019] The corrosion rates of the overhead lines of a benzene drying and light ends removal tower of the type shown in Fig. 1 were taken. The overhead pH ranged from about 1-7 in the overhead and under the C-l corrosion treatment program, corrosion rates of up to 300 mpy were experienced. When the pH approached about 2, the C-l corrosion inhibitor could not control corrosion. The Ex-1 corrosion inhibition treatment was initiated and corrosion rates of about 0.1 mpy were experienced then even at pH of about 2.
[0020] The description provided hereinabove is intended to generally describe the features and some useful embodiments of the invention. However, it will be appreciated that modifications may be made to many aspects of the invention without departing from its scope and generalized objects.
[0021] What is claimed is:

Claims

1. Method of inhibiting corrosion of metal surfaces in contact with a corrosive acidic medium comprising adding to said corrosive acidic medium, an effective amount of an ASA.
2. Method as recited in claim 1 wherein from about 1-500 ppm of said ASA is added to said corrosive acidic medium based upon 1 million parts of said corrosive acidic medium.
3. Method as recited in claim 2 wherein said ASA is devoid of nitrogen.
4. Method as recited in claim 3 wherein said ASA is a reaction product of C8-C32 olefin or mixture thereof with an unsaturated acidic reagent.
5. Method as recited in claim 4 wherein said unsaturated acidic reagent comprises maleic acid or anhydride.
6. Method as recited in claim 5 wherein said olefin is C12, C16, or C18, or mixtures thereof.
7. Method as recited in claim 1 wherein said corrosive acidic medium comprises HC1 and benzene therein and has a pH of about 1-7.
8. Method as recited in claim 7 wherein said corrosive acidic medium has a pH of about 2.0 or less.
9. Method as recited in claim 1 wherein said corrosive acidic medium is present in an overhead section of a benzene drying tower of the type adapted to purify benzene for feed of said purified benzene to a reactor employing a zeolite catalyst.
10. Method as recited in claim 9 wherein said reactor is a benzene alkylation reactor adapted to form ethyl benzene (EB) from said purified benzene and ethene, wherein said benzene and said ethene contact said zeolite catalyst.
11. Method as recited in claim 9 wherein said reactor is a benzene alkylation reactor adapted to form cumene from said purified benzene and propylene, wherein said benzene and propylene contact said zeolite catalyst.
12. Method as recited in claim 10 wherein said ASA is devoid of nitrogen.
13. Method as recited in claim 10 wherein said ASA is a reaction product of C8-C32 olefin or mixtures thereof with an unsaturated acidic reagent.
14. Method as recited in claim 13 wherein said unsaturated acidic reagent comprises maleic acid or anhydride.
15. Method as recited in claim 14 wherein said ASA is C12, C16, or C18 or mixtures thereof.
16. Method as recited in claim 15 wherein said corrosive acidic medium comprises water, HC1 and benzene therein and has a pH of about 1-7.
17. Method as recited in claim 15 wherein said corrosive acidic medium has a pH of about 2.0 or less.
18. Method as recited in claim 13 wherein said corrosive acidic medium is in gas phase.
PCT/US2012/067011 2012-11-29 2012-11-29 Alkenyl succinic acids or anhydrides as corrosion inhibitors for metal surfaces WO2014084828A1 (en)