WO1993018090A1 - Ignition resistant polycarbonate blends - Google Patents

Ignition resistant polycarbonate blends Download PDF

Info

Publication number
WO1993018090A1
WO1993018090A1 PCT/US1993/002111 US9302111W WO9318090A1 WO 1993018090 A1 WO1993018090 A1 WO 1993018090A1 US 9302111 W US9302111 W US 9302111W WO 9318090 A1 WO9318090 A1 WO 9318090A1
Authority
WO
WIPO (PCT)
Prior art keywords
composition
copolymer
polycarbonate
parts
tetrafluoroethylene
Prior art date
Application number
PCT/US1993/002111
Other languages
French (fr)
Inventor
Samuel A. Ogoe
Michael K. Laughner
Jack W. Muskopf
Jeffrey Earl Lackey
Thoi Huu Ho
Original Assignee
The Dow Chemical Company
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Priority claimed from US07/850,323 external-priority patent/US5258432A/en
Application filed by The Dow Chemical Company filed Critical The Dow Chemical Company
Publication of WO1993018090A1 publication Critical patent/WO1993018090A1/en

Abstract

A composition containing polycarbonate blended with one or more other polymers such as polyester, an acrylate polymer, a vinyl aromatic copolymer or a polyolefin, modified with poly(tetrafluoroethylene), an organophosphorous compound and optionally an aromatic halogenated carbonate oligomer to obtain ignition resistance properties, optionally further modified with a fine, free-flowing powder as a dispersing agent to improve surface properties, and, optionally, containing an elastomeric impact modifier.

Description

IGNITION RESISTANT POLYCARBONATE BLENDS
This invention relates to ignition resistant blended compositions of polycarbonate with one or more other polymers such as polyester, an acrylate polymer, a vinyl aromatic copolymer or a polyolefin, and to methods of preparation of such compositions.
Although many flame and ignition retardants for thermoplastics are known, it has been found to be preferred, in a blend of polycarbonate with one or more other polymers such as polyester, an acrylate polymer, a vinyl aromatic copolymer or a polyolefin, to thoroughly disperse ignition resistance additives in the polycarbonate composition, and to avoid the use of flame retardants which could cause transesterification of polycarbonate and polyester, or could otherwise cause degradation of the polycarbonate composition.
In one aspect, this invention involves a composition of matter containing, in admixture, (a) polycarbonate, (b) one or more members of the group consisting of polyester, an acrylate polymer, a vinyl aromatic copolymer and a polyolefin, (c) fibril-forming
poly(tetrafiuoroethylene), (d) an organophosphorous compound, and (e) a free-flowing, powdered dispersing agent having an average particle size less than 1 ,000 microns.
In another aspect, this invention involves a method of preparing a blended polycarbonate composition which comprises, in admixture, (a) polycarbonate, (b) one or more members of the group consisting of polyester, an acrylate polymer, a vinyl aromatic copolymer and a polyolefin, (c) fibril-forming poly(tetrafluoroethylene), (d) an organophosphorous compound, and (e) a free-flowing, powdered dispersing agent having an average particle size less than 1,000 microns; said method comprising (I) first forming a pre-mixture containing component (c), the fibril-forming poly(tetrafluoroethylene), and component (e), the dispersing agent, and (II) blending components (a), (b) and (d) with said pre-mixture.
In yet another aspect, this invention involves a composition of matter containing, in admixture, polycarbonate, polyester, fibril-forming poly(tetrafluoroethylene), an organophosphorous compound, and an aromatic halogenated carbonate oligomer. In a further aspect, this invention involves a composition of matter containing, in admixture, polycarbonate, an acrylate polymer, fibril-forming poly(tetrafluoroethylene), an
organophosphorous compound, and an aromatic halogenated carbonate oligomer.
It has been found that articles molded from the compositions of this invention exhibit advantageous levels of ignition and impact resistance, and are characterized by desirable surface aesthetics.
The compositions of this invention are useful, for example, in the production of films, fibers, extruded sheets, multi-layer laminates and molded or shaped articles of virtually all varieties, especially data storage apparatus, appliance and instrument housings, motor vehicle body panels and other parts and components for use in the automotive, electrical and electronics industries. The methods of this invention are useful for preparing compositions and molded articles having applications which are the same as or similar to the foregoing.
The compositions of this invention include those in which (a) a blend of (i) polycarbonate with one or more members of the group consisting of (ii) polyester, (iii) an acrylate polymer, (iv) a vinyl aromatic copolymer, and (v) a polyolefin, has been admixed in a composition with (b) (i) an organophosphorous compound, (ii) fibril-forming
poty(tetrafluoroethylene), and (iii) a dispersing agent. The compositions of this invention may, optionally, contain (c) an elastomeric impact modifier- Suitable ranges of content for components
(a) - (c) in the compositions of this invention, expressed in parts by weight of the total composition, are as follows:
(a) (0 polycarbonate from about 5 parts to about 95 parts, and preferably from about 25 parts to about 80 parts,
(a) (ii) polyester up to about 80 parts, preferably from about 10 parts to about
70 parts, and more preferably from about 20 parts to about 70 parts,
(a) (iii) acrylate polymer up to about 80 parts, preferably from about 10 parts to about 70 parts, and more preferably from about 20 parts to about 70 . parts,
(a) (iv) vinyl aromatic copolymer up to about 80 parts, preferably from about
10 parts to about 70 parts, and more preferably from about 20 parts to about 70 parts,
(a) (v) polyolefin up to about 80 parts, preferably from about 10 parts to
about 70 parts, and more preferably from about 20 parts to about 70 parts,
(b) (i) organophosphorous compound from about 0.001 part to about 20
parts, and preferably from about 0.1 part to about 10 parts,
(b) (ii) fibril-forming poly(tetrafluoroethylene) from about 0.001 part to
about 20 parts, preferably from about 0.01 part to about 10 parts, and more preferably from about 0.1 part to about 5 parts,
(b) (iii) dispersing agent from about 0.001 part to about 50 parts, preferably from about 0.1 part to about 30 parts, and more preferably from about 0.1 part to about 20 parts, and
(c) elastomeric impact modifier up to about 30 parts, preferably from
about 1 to about 20 parts, and preferably from about 1 to about 15 parts.
The compositions of this invention also include those in which (d) a blend of (i) polycarbonate and (ii) polyester and/or (iii) an acrylate polymer has been admixed in a composition with (e) (i) an organophosphorous compound, (ii) fibril-forming poly(tetrafluoroethylene), and (iii) a halogenated aromatic carbonate oligomer. The compositions of this invention may, optionally, contain (f) an elastomeric impact modifier. Suitable ranges of content for components (d) - (f) in the compositions of this invention, expressed in parts by weight of the total composition, are as follows:
(d) (i) polycarbonate from about 5 parts to about 95 parts, and preferably from about 25 parts to about 80 parts,
(d) (ii) polyester up to about 80 parts, preferably from about 10 parts to about
70 parts, and more preferably from about 20 parts to about 70 parts,
(d) (iii) acrylate polymer up to about 80 parts, preferably from about 10 parts to about 70 parts, and more preferably from about 20 parts to about 70 parts,
(e) (i) organophosphorous compound from about 0.001 part to about 20 parts, preferably from about 0.1 part to about 10 parts, and more preferably from about 0.1 part to about 5 parts,
(e) (ii) fibril-forming poly(tetrafluoroethylene) from about 0.001 part to about 20 parts, preferably from about 0.01 part to about 10 parts, and more preferably from about 0.1 part to about 5 parts,
(e) (iii) halogenated aromatic carbonate oligomer from about 0.001 part to about 50 parts, preferably from about 0.1 part to about 30 parts, and more preferably from about 0.1 part to about 20 parts,
(f) elastomeric impact modifier up to about 30 parts, preferably from about 1 to about 20 parts, and preferably from about 1 to about 15 parts.
Preparation of the compositions of this invention can be accomplished by any suitable mixing means known in the art. Typically the substances to be admixed with the polycarbonate/polyester blend are dry blended in particulate form with sufficient agitation to obtain thorough distribution thereof. If desired, the dry-blended formulation can further be melt mixed, for example in an extruder with or without a vacuum, or otherwise compounded with additional substances. Apparatus which can be used in the blending process include, for example, mixing rolls, a dough-mixer or a Banbury mixer.
Methods for preparing the compositions of this invention also involve pre-mixing the poly(tetrafluoroethylene) ("PTFE"), component (b)(ii), with the dispersing agent, component(b)(iii), before either of them is mixed with any of the other components of the composition. This pre-mixing prevents the presence of the PTFE from causing the surface of an article molded from a composition of the invention to show streaks or different degrees of shading or coloration, which gives an appearance very similar to that of grain in wood.
When softened or melted by the application of heat, the compositions of this invention can undergo fabrication and can therein be formed or molded using conventional techniques such as compression, injection molding, gas assisted injection molding, calendering, vacuum forming, thermoforming, extrusion and/or blow molding techniques, alone or in combination. The compositions can also be formed, spun or drawn into films, fibers, multilayer laminates or extruded sheets, or can be compounded with one or more organic or inorganic substances, on any machine suitable for such purpose.
Articles molded from compositions prepared within the ranges of content stated above exhibit a desirably high level of ignition and impact resistance and are characterized by a surface which has uniform shading and shows no streaks or evidence of molding flow lines. When the composition contains the optional elastomeric impact modifier, impact resistance is further enhanced.
In a preferred embodiment, the compositions of this invention do not include an inorganic salt, particularly not an acidic or basic inorganic salt. Inorganic salts are, in general, those which do not contain carbon, and, in particular, do not contain an aromatic ring.
Representative examples of inorganic salts which would, in such preferred embodiment, not be included in a composition of this invention are those formed from antimony, an alkali metal or alkaline earth metal and a counterion containing nitrogen, sulfur, phosphorous and/or oxygen. Specific examples of such salts are antimony oxide, Na2SO4, K2SO4 and NaHSO4. Salts such as the aforementioned could cause degradation and/or transesterfication of the polycarbonate and polyester resins, and their presence therefore may not be desirable in the compositions of this invention. However, compositions of the invention may or may not include organic salts.
Component (a)(i) and (d)(i) in the compositions of this invention is a polycarbonate, which can be prepared from a dihydroxy compound such as a bisphenol, and a carbonate precursor such as a disubstituted carbonic acid derivative, a haloformate (such as a bishaloformate of a glycol or dihydroxy benzene) or a carbonate ester. These components are often reacted by means of the phase boundary process in which the dihydroxy compound is dissolved and deprotonated in an aqueous alkaline solution and the carbonate precursor is dissolved in an organic solvent. The aqueous alkaline solution has a pH of 7.01 or more and can be formed in water from a caustic soda, such as NaOH, or from other bases such as those included in the alkali metal and alkaline earth metal phosphates, bicarbonates, oxides and hydroxides. These components are often reacted by means of a mixture prepared initially from the aromatic dihydroxy compound, water and a non-reactive organic solvent immiscible with water selected from among those in which the carbonate precursor and polycarbonate product are soluble. Representative solvents include chlorinated hydrocarbons such as methylene chloride, 1,2-dichloroethane, tetrachloroethane, chlorobenzene, and chloroform, to which tetrahydrofuran, dioxane, nitrobenzene, dimethyl sulfoxide, xylene, cresol or anisole may be added, if desired. Caustic soda or other base is then added to the reaction mixture to adjust the pH of the mixture to a level at which the dihydroxy compound is activated to dianionic form. A reducing agent such as sodium sulfite or sodium dithionite can also be advantageously added to the reaction mixture as well.
A carbonate precursor is contacted with an agitated mixture of the aqueous alkaline solution of the dihydroxy compound, and, for such purpose, the carbonate precursor can be bubbled into the reaction mixture in the form of a gas, or can be dissolved and introduced in solution form. The mixture is agitated in a manner which is sufficient to disperse or suspend droplets of the solvent containing the carbonate precursor in the aqueous alkaline solution. Reaction at the interface of the organic and aqueous phases created by such agitation yields the bis(carbonate precursor) ester of the dihydroxy compound. For example, if the carbonate precursor is a carbonyl halide such as phosgene, the products of this initial phase of the process are monomers or oligomers which are either mono- or dichloroformates, or contain a phenolate ion at each terminus. These intermediate mono- and oligocarbonates dissolve in the organic solvent as they form, and they can then be condensed to a higher molecular weight polycarbonate by contact with a coupling catalyst of which the following are representative: a tertiary amine such as triethyl amine or dimethyl amino pyridine; a hindered secondary amine such as diisopropyl amine; a cyclic aza compound such as 2,2,6,6-tetramethyl piperidine or 1,2-dimethylimidazole; an amidine or aminoamidine compound such as 1-methyl-2-phenyliminopyrrolidine; an isourea compound such as N,N-dibutyl-N'-phenyl-o-methylisourea; an imino ether or imino carboxylate compound such as 1-aza-2-methoxy-1-cycloheptene or t-butyl-cyclohexyliminoacetate; or a phosphonium, sulfonium, arsonium or quaternary ammonium compound. Such a catalyst may be added to the reaction mixture before or after it is contacted with a carbonate precursor.
The reaction can be run at a pH of 7.01 to 14, and at a temperature between 0°C-100°C, although usually not in excess of the boiling point (reflux temperature) of the solvent used. Frequently, the reaction is run at a temperature of about 0°C to about 45°C.
Upon completion of polymerization, the organic and aqueous phases are separated to allow purification of the organic phase and recovery of the polycarbonate product therefrom. The organic phase is washed as needed in a centrifuge with dilute base, water and/or dilute acid until free of unreacted monomer, residual process chemicals and/or other electrolytes. Recovery of the polycarbonate product can be effected by spray drying, steam devolatilization, direct devolatilization in a vented extruder, or precipitation by use of an anti-solvent such as toluene, cyclohexane, heptane, methanol, hexanol, or methyl ethyl ketone.
In the melt process for preparation of polycarbonate, aromatic diesters of carbonic acid are condensed with an aromatic dihydroxy compound in a transesterification reaction in the presence of a basic catalyst such as sodium methylate, sodium bisphenolate, calcium acetate, phenyl benzoate, N-stearoylphenothiazine, quaternary ammonium chloride, an alkaline(hydroxy)fluoroborate, an alkali metal salt of benzoic acid, an imino carboxylic acid, or basic metal oxides such as zinc, lead or antimony oxide. The reaction is typically run at 250°C-300°C under vacuum at a progressively reduced pressure of 1-100 mm Hg. The reaction is run in the absence of solvent and typically yields lower viscosity grades of polycarbonate.
Polycarbonate can also be prepared in a homogeneous solution through a process in which a carbonate precursor, such as phosgene, is contacted with a solution containing an aromatic dihydroxy compound, a chlorinated hydrocarbon solvent and a substance, such as pyridine, dimethyl aniline or CaOH, which acts as both acid acceptor and condensation catalyst. Washing with acidified water removes the pyridine and its hydrochloride, and precipitation and repulping with an antisol vent such as heptane followed by filtration and distillation removes oligomers and unreacted monomer.
Yet another process for the preparation of polycarbonate is the polymerization of cyclic oligomers having a weight average molecular weight of approximately 1,300 at 200°C-300°C, using a catalyst such as lithium stearate or tetramethylammonium tetraphenylborate.
Examples of some dihydroxy compounds suitable for the preparation of polycarbonate include variously bridged, substituted or unsubstituted aromatic dihydroxy compounds (or mixtures thereof) represented by the formula
Figure imgf000008_0001
wherein:
(I) Z is (A) a divalent radical, of which all or different portions can be (i) linear,
branched, cyclic or bicyclic, (it) aliphatic or aromatic, and/or (iii) unsaturated, said divalent radical being composed of 1-35 carbon atoms together with up to five oxygen, nitrogen, sulfur, phosphorous and/or halogen (such as fluorine, chlorine and/or bromine) atoms; or (B) S, S2, SO, SO2, O or CO; or (C) a single bond; and
(II) each X is independently hydrogen, a halogen (such as flourine, chlorine and/or bromine), a C1-C12 linear or cyclic alkyl, alkoxy, aryl or aryloxy radical, such as methyl, ethyl, isopropyl, cyclopentyl, cyclohexyl, methoxy, ethoxy, benzyl, tolyl, xylyl, phenoxy and/or xylynoxy.
For example, the bridging radical represented by Z in the above formula can be a carbon atom to which is bonded one or more groups such as CH3, C2H5, C3H7, n-C3H7, i-C3H7, cyclohexyl, bicyclo[2.2.1]heptyl, benzyl, CF2, CF, CCl3, CF2Cl, CN, (CH2)2COOCH3, or PO(OCH3)2.
Representative examples of dihydroxy compounds of particular interest are 2,2-bis(4-hydroxyphenyl)propane ("Bisphenol-A" or "Bis-A");
2,2-bis(3,5-dihalo-4-hydroxyphenyl)propane ("Tetrahalo Bisphenol-A") where the halogen can be fluorine, chlorine, bromine or iodine, for example 2,2-bis(3,5-dibromo-4-hydroxyphenyl)propane ("Tetrabromo Bisphenol-A" or "TBBA");
2,2-bis(3,5-dialkyl-4-hydroxyphenyl)propane ("Tetraalkyl Bisphenol-A") where the alkyl can be methyl or ethyl, for example 2,2-bis(3,5-dimethyl-4-hydroxyphenyl)propane ("Tetramethyl Bisphenol-A");
1,1-bis(4-hydroxyphenyl)-1-phenyl ethane ("Bisphenol-AP" or "Bis-AP");
Bishydroxy phenyl fluorene.
Using a process such as is generally described above, a polycarbonate product can be obtained having a weight average molecular weight, as determined by light scattering or gel permeation chromatography, of 8,000 to 200,000 and preferably 15,000 to 40,000, although values outside these ranges are permitted as well. Molecular weight can be controlled by addition to the reaction mixture of a chain terminator which may be selected from monofunctional substances such as phenols, alcohols, amines, imides, carbonic acid chlorides, sulfonic acid chlorides, benzyltriethyl ammonium chloride, or
phenylchlorocarbonates. A chain terminator may be added to the reaction mixture before or after a dihydroxy compound is contacted with a carbonate precursor.
A branched rather than linear polycarbonate molecule can be obtained by adding to the reaction mixture a tri- or polyfunctional monomer such as a tri- or tetrafunctional phenol or carboxylic acid (or a derivative such as an acyl halide or anhydride), a bisphenol containing carboxylic acid side groups, or a nitrogen-containing compound such as cyanuric chloride, or compounds containing a mixture of such groups. Preferred branching agents are trimellitic acid or pyromellitic dianhydride.
The preferred process of this invention is that in which an aromatic polycarbonate is prepared. An aromatic polycarbonate is defined herein with reference to the oxygen atoms, of the one or more dihydroxy compounds present in the polycarbonate chain, which are bonded to a carbonyl carbon. In an aromatic polycarbonate, all such oxygen atoms are bridged by a dihydroxy compound residue some portion of which is an aromatic ring.
Also included within the term "polycarbonate", as used herein, are various copolycarbonates, certain of which can be prepared by incorporating one or more different dihydroxy compounds into the reaction mixture. This can be accomplished by charging the dihydroxy compounds themselves to the reaction mixture either simultaneously or
sequentially. If the dihydroxy compounds are added sequentially or added together but have different reactivities toward the carbonate precursor, a segmented or block copolycarbonate will typically result. Different dihydroxy compounds with the same reactivity typically yield a random copolycarbonate when reacted together. Alternatively, if oligocarbonates are formed separately from one or more different dihydroxy compounds, the oligocarbonates can then be coupled in a condensation reaction to yield a segmented or block copolycarbonate. When a dicarboxylicacid (or derivative) or a hydroxycarboxylic acid is used in the reaction mixture, or to form an oligomeric prepolymer, instead of one of the different dihydroxy compounds mentioned above, a poly(ester/carbonate) is obtained.
Copolycarbonates can also be prepared, for example, by reaction of one or more dihydroxy compounds with a carbonate precursor in the presence of a chlorine- or amino-terminated polysiloxane, with a hydroxy-terminated poly(phenylene oxide) or poly(methyl methacrylate),or with phosphonyl dichloride or an aromatic ester of a phosphonic acid.
Siloxane/carbonate block copolymers are discussed in greater detail in Paul, U.S. Pat. No.
4,596,970 and poly(ester/carbonate)s are discussed in greater detail in Swart, U.S. Pat. No. 4,105,533, each of which is incorporated herein.
The methods generally described above for preparing carbonate polymers suitable for use in the practice of this invention are well known; for example, several methods are discussed in detail in Schnell, USP 3,028,365; Campbell. USP 4,384,108; Glass, USP 4,529,791; and Grigo, USP 4,677, 162, each of which is incorporated as a part hereof.
Component (a)(ii) and (d)(ii) in the compositions of this invention is a polyester, which may be made by the self-esterification of hydroxycarboxylic acids, or direct esterification, which involves the reaction of a diol with a dicarboxylic acid with the resulting elimination of water, giving an -[-AABB-]- polyester. Temperatures applied exceed the melting points of the reactants and typically approach the boiling point of the diol being used, and usually range from about 150°C to about 280°C. An excess of the diol is typically used, and once all of the acid has reacted with diol, the excess diol is removed by distillation with the application of additional heat under reduced pressure.
Alternatively, but in like manner, ester-forming derivatives of a dicarboxylic acid can be heated with a diol to obtain polyesters in an ester interchange reaction. Suitable acid derivatives for such purpose are esters, halides, salts or anhydrides of the acid. The ester interchange reaction is typically run in the presence of a diluent, for example, an inert organic solvent such as chloroform or tetrachloroethane, and in the presence of a base, for example a tertiary organic base such as pyridine. Typical catalysts used when ester interchange involves alcoholysts are weak bases such as carbonates or alkoxides of sodium, lithium, zinc, calcium, magnesium or aluminum, whereas catalysts such as antimony oxide, titanium butoxide or sodium acetate are often used when acidolysis occurs in the interchange reaction. Diol derivatives such as an acetate can be used effectively when it is desired to conduct acidolysis.
The molecular weight of polyester can be increased by adding a chain coupling agent, such as diphenyl carbonate, to the melt reaction mixture just prior its completion. Or, to achieve higher weight by solid state polymerization, polyester product of intermediate weight can be heated in a vacuum or stream of inert gas, first to a temperature where it crystallizes and then to a temperature close to its melting point. Polyesters can also be produced by a ring-opening reaction of cyclic esters or lactones, for which organic tertiary bases and alkali and alkaline earth metals, hydrides and alkoxides can be used as initiators.
Whether a polyester is crystalline or amorphous is typically a function of the symmetry of the starting materials from which it is made. When one or more hydrogens on the diol and/or the diacid (or derivative) which are reacted to form a polyester are replaced by larger radicals such as alkyl or halogen, the intermolecular spacing of the resulting molecules may be disrupted if the presence of the substituent creates asymmetric or irregularly shaped molecules. The component containing the substituent may also be combined into the polyester molecule in random orientation, resulting in structural irregularity in the polymer chain. Factors which can influence crystallization of ring-containing polyesters are the directionality of the ester groups, the stereochemistry of the rings and variations in symmetry where the rings are bridged. For example, a poly(alkylene isophthalate) crystallizes only with difficulty, and a polyester prepared from phthalic acid typically does not crystallize at all.
However, where the amount of monomer containing the asymmetry is small in relation to the remainder of the starting materials, the portion of the resulting polyester molecule which suffers from structural irregularity will also be small, and crystallization will typically not be impeded. A crystalline material may be identified by the endotherm it displays on a differential scanning calorimeter. A preferred polyester for use in this invention is a crystalline polyester having a melting point of 254-260°C.
Suitable reactants for making the polyester used in this invention, in addition to hydroxycarboxylic acids, are diols and dicarboxylic acids either or both of which can be aliphatic or aromatic. A polyester which is a poly(alkylene alkanedicarboxylate), a poly(alkylene phenylenedicarboxylate), a poly(phenylene alkanedicarboxylate), or a poly(phenylene phenylenedicarboxylate) is therefore appropriate for use herein. Alkyl portions of the polymer chain can be substituted with, for example, halogens, alkoxy groups or alkyl side chains and can contain divalent heteroatomic groups (such as -O-, -S- or -SO2-) in the paraffinic segment of the chain. The chain can also contain unsaturation and non-aromatic rings. Aromatic rings can contain substituentssuch as halogens, alkoxy or alkyl groups, and can be joined to the polymer backbone in any ring position and directly to the alcohol or acid functionality or to intervening atoms.
Typical alkylene diols used in ester formation are the C2-C10 glycols, such as ethylene-, propylene-, and butylene glycol. Alkanedicarboxylic acids frequently used are oxalic acid, adipic acid and sebacic acid. Diols which contain rings can be, for example, a 1,4-cyclohexyl enyl glycol or a 1 ,4-cyclohexane-dimethylene glycol, resorcinol, hydroquinone, 4,4'-thiodiphenol, bis-(4-hydroxyρhenyl)sulfone, a dihydroxynaphthalene, a xylylene diol, or can be one of the many bisphenols such as 2,2-bis-(4-hydroxyphenyl)propane. Aromatic diacids include, for example, terephthalic acid, isophthalic acid, naphthalenedicarboxylic acid, diphenyletherdicarboxylic acid, diphenyldicarboxylic acid, diphenylsulfonedicarboxylic acid, diphenoxyethanedicarboxylicacid.
In addition to polyesters formed from one diol and one diacid only, the term "polyester" as used herein includes random, patterned or block copolyesters, for example those formed from two or more different diols and/or two or more different diacids, and/or from other divalent heteroatomic groups. Mixtures of such copolyesters, mixtures of polyesters derived from one diol and diacid only, and mixtures of members from both of such groups, are also all suitable for use in this invention, and are all included in the term "polyester". For example, useof cyclohexanedimethylol together with ethylene glycol in esterification with terephthalic acid forms a clear, amorphous copolyester ("PETG") of particular interest. Also contemplated are PCTG; liquid crystalline polyesters derived from mixtures of 4-hydroxybenzoic acid and 2-hydroxy-6-naphthoic acid; or mixtures of terephthalic acid, 4-hydroxybenzoic acid and ethylene glycol; or mixtures of terephthalic acid, 4-hydroxybenzoic acid and 4,4'-dihydroxybiphenyl.
Aromatic polyesters, those prepared from an aromatic diacid, such as the poly(alkylene phenylenedicarboxylates) polyethylene terephthalate and polybutylene terephthalate, or mixtures thereof, are particularly useful in this invention.
Methods and materials useful for the production of polyesters, as described above, are discussed in greater detail in Whinfield, US Pat. No.2,465,319, Pengilfy, US Pat. No. 3,047,539 and Russell, US Pat. No.3,756,986, each of which is incorporated herein by reference.
Component (a)(iii) and (d)(iii) in the compositions of this invention is an acrylate polymer, which is defined as a polymer prepared by homopolymerization of an alkyl acrylate or an alkyl methacrylate or by copolymerization of a mixture of the two; and includes a mixture of any such homopolymers or copolymers.
An alkyl acrylate or methacrylate can be prepared, for example, by reaction of an alkyl alcohol or diazoalkane with acrylic or methacrylic acid. Acrylic acid is prepared by the vapor phase oxidation of propylene. The acrylic acid/alcohol esterification reaction can be run at about 80°C using an acid catalyst such as H2SO4. Methacrylic acid may be prepared bythe oxidation of isobutylene ort-butyl alcohol. A methacrylate may also be prepared by reacting acetone cyanohydrin with an excess of concentrated sulf uric acid to form methacrylamide sulfate, which, when then reacted with an alcohol, yields a methacrylate. A C1 - C10 acrylate or methacrylate may be used for polymer preparation herein, with C1- C6 acrylate or methacrylate being preferred, and C1 - C4 being more preferred.
The acrylate polymer used in the compositions of this invention can be prepared in a polymerization reaction initiated by free radical initiators such as azo compounds or peroxides, preferably in the absence of oxygen. Methacrylate monomers are most often polymerized in bulk, but this method has little application for acrylate monomers. Acrylate and methacrylate monomers may be polymerized in an organic solution, using, for example, an aromatic hydrocarbon, ester, ketone or chlorohydrocarbon (such as toluene, chlorobenzene or 3-pentanone) as the solvent. A chain transfer agent such as a thiol may be used to control molecular weight. Polymerization can also occur in an aqueous emulsion in which an anionic surfactant, such as ah alkylarene sulfate or phosphate, a nonionic surfactant, such as an alkyl or aryl polyoxyethylene, or a cationic surfactant is used. Suspension polymerization is used primarily for methacrylates and involves suspending in water 0.1-5 mm droplets of monomer which are stabilized by a protective colloid such as cellulose, poly(vinyl alcohol), gelatin or talc. The initiator should be soluble in the monomer but not in water. Acrylates and methacrylates can also be polymerized in a non-aqueous dispersion using an organic diluent such as hexane or methanol.
When an acrylate and a methacrylate are copolymerized, the acrylate, each can be used in the mix of reactants from which the copolymer results in an amount of up to about 99.0 parts by weight, based on the total weight of the copolymer. When the acrylate polymer takes the form of a copolymer, the copolymer may be a random, alternate, block or grafted copolymer.
Component (a)(iv) in the compositions of this invention is a vinyl aromatic copolymer prepared from a vinyl aromatic compound and one or more copolymerizable, ethylenically unsaturated monomers. The vinyl aromatic copolymer may be a random, alternate, block or grafted copolymer, and a mixture of more than one vinyl aromatic copolymer may be used as well. Ethylenically unsaturated monomers of particular interest for copolymerization with a vinyl aromatic compound include a vinyl nitrile compound, a diene, an alkyl or aryl acrylate or methacrylate, glycidyl methacrylate, an alkyl or aryl maleate or fumarate, the anhydride of an unsaturated carboxylic acid such as maleic anhydride, an alkyl or aryl maleimide, ethyl ene/propylene/diene copolymer, and an oxazoline compound.
In addition to other particular species of various ethylenicaliy unsaturated monomers which are noted below in the discussion of producing
acrylonitrile/butadiene/styrene copolymer ("ABS"), the category of vinyl aromatic compounds includes styrene and substituted styrenes; vinyl nitrile compounds include acrylonitrile and substituted acrylonitriles; alkyl acrylates and methacrylates include C1 - C10 acrylates and methacrylates; alkyl or aryl maleimide compounds include the reaction product of a C1 - C10 alkyl or C6 - C14 aryl primary amine and maleic anhydride; and an oxazoline compound includes those of the general formula
Figure imgf000014_0001
where each J is independently hydrogen, halogen, a C1-C10 alkyl radical or a C6-C14 aryl radical.
The preferred vinyl aromatic copolymer is a rubber-modified vinyl aromatic/vinyl nitrile copolymer. The rubber content of a rubber-modified vinyl aromatic copolymer employed in the compositions of this invention is about 5 to about 50 percent by weight. One example of a rubber-modified vinyl aromatic/vinyl nitrile copolymer is a rubber-modified styrene/acrylonitrile copolymer ("SAN") such as ABS. ABS, an elastomeric-thermoplastic composite, is typically formed by the grafting of an SAN copolymer onto a polybutadiene substrate latex. The polybutadiene forms particles of rubber - the elastomeric component -which are dispersed as a discrete phase in a thermoplastic matrix formed by the SAN.
One method for making a vinyl aromatic copolymer is emulsion polymerization. For example, when ABS is made by emulsion polymerization, a rubber substrate latex is produced in an aqueous emulsion by a polymerization, which can be initiated by organic peroxides, persulfates or redox systems, of 1,3-butadiene alone or in combination with other diene monomers such as isoprene, 2,3-dimethyl butadiene-1 ,3 or piperylene, or a combination of two or more of these and a lesser amount of one or more of the following: vinyl aromatic monomers such as styrene, alpha-alkyl styrene, p-methoxy styrene, p-chloro styrene, dichloro styrene or vinyl naphthalene; vinyl nitrile monomers such as acrylonitrile, methacrylonitrile, ethacrylonitrile or alphachloro acrylonitrile; alkyl acrylates and methacrylates such as methyl acrylate, propyl acrylate, butyl acrylate, octyl acrylate, methyl alpha-chloro acrylate, methyl methacrylate, ethyl methacrylate or isobutyl methacrylate; methacrylamide oracrylamide, N,N-diethyl acrylamide; aliphatic or aromatic maleimides such as N-phenyl maleimide;
diethyichloromaleate; diethyl fumarate; vinylidene chloride; methyl vinyl ketone or methyl isopropenyl ketone; vinyl pyridines; vinyl furan; vinyl carbazole; isobutylene or ethylene; and the like. It is preferred that, in the preparation of the rubber latex, the proportion of butadiene to other monomers in the substrate latex be in the range of about 2/1 to about 15/1.
After formation of the rubber latex substrate, it is subjected to further aqueous emulsion polymerization with styrene and acrylonitrile monomers, wherein the concentration of styrene is usually about 1.5 to 3.5 times that of acrylonitrile. However, other monomers (including various vinyl aromatic or vinyl nitrile compounds) such as methacrylonitrile, divinylbenzene, α-methyl styrene, p-methyl styrene, methyl methacrylate, N-phenyl maleimide. chlorinated and brominated styrenes, and methyl-, ethyl- or n-butylacrylate, or mixtures thereof, may also be used in conjunction with styrene and acrylonitrile as the grafting monomers.
Organic peroxides, azo compounds, persulfates, or redox systems are usually used to initiate polymerization. SAN is formed, some of which is grafted to the rubber latex substrate, and some of which is free. The latex containing both the grafted rubber and the free SAN is then mixed with a coagulant solution, heated and agitated to produce discrete particles of ABS resin. The slurry containing those particles is dewatered in a centrifuge, and the resin is dried. Methods for making ABS resin by emulsion polymerization, as described above, are discussed in greater detail in Childers, USP 2,820,773 and Calvert, USP 3,238,275, each being hereby incorporated as a part hereof.
Another method for making a vinyl aromatic copolymer is suspension polymerization. For example, when ABS is made by suspension polymerization, a pre-formed elastomeric (rubber) component, usually a polybutadiene or a butadiene/styrene copolymer, is dissolved in a mixture of styrene and acrylonitrile. The rubber component may be one of the several mentioned above with respect to emulsion polymerization of ABS, or may be a diene such as polyisoprene, polycyclopentadiene, natural rubber, chlorinated rubber or copolymers of butadiene with isobutylene.
The preferred ratio of styrene to acrylonitrile in the styrene-acrylonitrile solution is about 90/10 to about 60/40, and in the preferred recipe the rubber component constitutes from about 4% to less than about 40% of the product. As with the emulsion process described above, numerous other vinyl aromatic compounds will function in a manner equivalent to that of styrene, to-wit: alphamethyl styrene, vinyl-toluene, vinylxylene, vinylethyl benzene or vinylchloro benzene. Methacrylonitrile is but one of many other other vinyl nitrile monomers which will serve in the place of, or in conjunction with, acrylonitrile.
The rubber component, monomers and initiator are charged to the reaction vessel and polymerization ensues until a conversion rate of about 15% to about 30% is reached, resulting in the production of a prepolymer. Phase inversion occurs, and the rubber precipitates from solution and becomes the discontinuous phase dispersed as particles ranging from 0.1 to 5 μm in size. The prepolymer is then placed in a suspension reactor in an aqueous solution containing a suspending agent, initiator and chain transfer agent. Typical suspending agents are carboxymethyl cellulose, polyvinyl alcohol, and polyglycol ethers. Typical initiators for the polymerization which occurs during suspension are t-butyl perbenzoate, di-t-butyl peroxide, or t-butyl peroxy isopropyl carbonate. Agitation of the solution completes the polymerization. The process is completed by dewatering the slurry in a centrifuge, and moisture content is further reduced by flash drying. Manufacture of ABS by the suspension process, as described above, is discussed in greater detail in Carrock, USP 3,515,692 and Ackerman, USP 4, 151,128, each being hereby incorporated as a part hereof. A third method for production of a vinyl aromatic copolymer is bulk or mass polymerization. For example, when ABS is made by bulk or mass polymerization, it is formed by dissolving an elastomeric (rubber) component in the monomer mix, which contains styrene, acrylonitrile, an initiator and, frequently, a chain transfer agent such as a mercaptan or a terpinolene. The reaction can, however, be thermally initiated. The styrene and acrylonitrile monomers polymerize, some grafting to the rubber component, but most forming a monomer-polymer solution. As the relative volume of the monomer-SAN polymer phase increases, discrete rubber particles become dispersed in the matrix resulting from the monomer-SAN polymer phase. The rubber particles are stabilized by being grafted to SAN polymers at the interface between the particles and the SAN polymer matrix. Additional stabilization is furnished when monomer becomes occluded, and polymerizes, within the rubber particles. Because polymerization occurs completely within a monomer/polymer medium, viscosity increases as conversion increases. To allow continued agitation of the reaction mixture despite such increasing viscosity, diluents such as methyl ethyl ketone and ethyl benzene are added to the reactor. Upon the completion of polymerization, the melt is devolatilized using equipment such as a devolatilizing extruder or a flash evaporator, and vacuum is applied to remove unreacted monomers and diluents.
As is true of a vinyl aromatic copolymer such as ABS made by the emulsion or suspension method, numerous substances can be used in the bulk method in place of, or conjunction with, styrene, examples of such substances being vinyl aromatic compounds as follows: alpha-methylstyrene, alpha-ethylstyrene, alpha-methylvinyltoluene; ring-substituted alkyl styrenes, e.g. vinyl toluene, o-ethylstyrene, p-ethylstyrene, 2,4-dimethylstyrene; ring-substituted halostyrenes, e.g., o-chlorostyrene, p-chlorostyrene, o-bromostyrene, 2,4-dichlorostyrene; ring-alkyl, ring-halo-substituted styrenes, e.g.2-chloro-4-methylstyrene and 2,6-dichloro-4-methylstyrene. Also useful are methacrylates such as methyl methacrylate; maleic acid and its esters and anhydrides; aliphatic or aromatic maleimides such as N-phenyl maleimide; and mixtures of any of the foregoing. Methacrylonitrile can also be used in combination with acrylonitrile. Bulk methods for the preparation of ABS, as described above, are discussed in greater detail in Kruse, USP 4,187,260, Simon, USP 4,252,911 and Weber, USP 4,526,926, each being hereby incorporated as a part hereof.
AES (acrylonitrile/EPDM/styrene) copolymer is a vinyl aromatic copolymer which is obtained when styrene/acrylonitrile copolymer is rubber-modified by grafting SAN to a substrate made up of an EPDM (ethylene/propylene/non-conjugated diene) rubber. AES copolymers are discussed in greater detail in Henton, USP 4,766,175, which is incorporated as a part hereof. SAN can also be crosslinked to an acrylate elastomer to form a vinyl aromatic copolymer, as in the case of an ASA (acrylonitrile/styrene/acrylate) copolymer, which is discussed in greater detail in Yu, USP 3,944,631 , which is also incorporated as a part hereof. Other vinyl aromatic copolymers of particular interest include aryl maleimimde/vinyl nitrile/diene/vinyl aromatic copolymer, vinyl aromatic/maleic anhydride copolymer, alkyl methacrylate/vinyl aromatic/vinyl nitrile copolymer, vinyl aromatic/alkyl methacrylate copolymer, vinyl aromatic/alkyl methacrylate/glydicyl methacrylate copolymer, vinyl aromatic/glydicyl methacrylate copolymer, styrene/butyl acrylate copolymer, methyl methacryalte/acrylonitrile/butadiene/styrene copolymer and phenyl
maleimide/acrylonitrile/butadiene/styrene copolymer.
Component (a)(v) in the compositions of this invention is a polyolefin. A polyolefin may be any of the several different kinds mentioned below including, for example, linear low density polyethylene ("LLDPE"). LLDPE is formed under the kind of low pressure conditions which are usually employed for forming high density polyethylene ("HDPE").
However, a low density product (0.910 - 0.940 g/cm3) results because, rather than forming a homopolymer, ethylene is copolymerized with one or more α-olefins, which in the final product take on the form and function of short side chains. Because the comonomers most frequently used are α-olefins such as 1-butene, 4-methyl-1-pentene, 1-hexene or 1-octene, these side chains do prevent the close, fully crystalline type of packing representative of HDPE, but they are not nearly as long as the fully branched, long side chains associated with low density polyethylene ("LDPE") made under high pressure conditions.
LLDPE can be formed in a slurry using a light hydrocarbon diluent and a supported chromium catalyst, or it can be formed as a slurry in hexane using organometal-titanium type catalysts. It can also be formed in cyclohexane in solution at a relatively high temperature, approximately 250°C, using as a catalyst a combination of tri butyl aluminum, titanium tetrachloride and vanadium oxychloride. LLDPE can also be formed in gas phase using a fluidized bed of growing polymer particles to which a supported chrominum oxide catalyst modified with titanium and fluoride is charged, as described in Levine, USP 4,011 ,382
(incorporated herein), or by a gas-phase process using a stirred but non-fluidized bed and a supported titanium catalyst-triethylaluminum cocatalyst as described in Jezl, USP 4,129,729 (incorporated herein).
LDPE is typically thought of as that which is made under high pressure conditions and has a density between about 0.916 to about 0.930 g/cm3. This low density results from the many zones of amorphous arrangement which are characteristic of LDPE because of its long chain branches, which can contain thousands of carbon atoms. LDPE can be made in either a tubular reactor or a stirred autoclave, where heated, pressurized feed streams of ethylene gas, peroxide free-radical initiator and chain transfer agent are injected into the reaction device. The reaction of formation usually occurs at 1,500-3,000 atm (152-304 MPa) and at a temperature usually not exceeding 300°C, as known in the art. LDPE can be copolymerized with monomers such vinyl acetate, ethyl acrylate, acrylic acid or other polar vinyl monomers.
An HDPE homopolymer is typically about 94% crystalline and has a density of about 0.950 to about 0.970 g/cm3. HDPE, because of its much greater crystallinity and density, has a higher melting point than LDPE - 135°C vs. 115°C. The molecular weight of HDPE usually ranges from 50,000 to 1,000,000 or more. One process for making HDPE involves
polymerization at about 100-150°C and atabout2-4MPa (290-580 psi) using a chromium oxide-promoted silica catalyst- HDPE is also manufactured in a slurry system wherein high purity ethylene is fed to a loop reactor which contains a low boiling hydrocarbon used to dissolve the ethylene, and to suspend the catalyst and polymer particles. The temperature is typically between about 70-110°C and the pressure is typically between about 1 and 5 MPa. A chromium catalyst on a powdered silica substrate is typically used. As the polymer particles are formed they are removed from the reactor in a concentrated slurry and are discharged into a flash tank for drying. Alternatively, HDPE can be made in a gas-phase process wherein no hydrocarbon diluent is used and a fluidized bed is used to agitate and suspend the polymer particles.
Methods for making HDPE are more particularly described in Hogan, USP 2,825,721
(incorported herein).
Ziegler process polyethylene ("ZPE") has great versatility because of the wide range of molecular weights in which it can be prepared using the versatile Ziegler catalyst. ZPE can include, for example, waxes ranging in molecular weight from 10,000 to ultrahigh molecular weight HDPE having a molecular weight of several million. ZPE has a density of about 0.940 to about 0.965 g/cm3. Both supported and non-supported magnesium-titanium catalyst systems find wide use in the manufacture of ZPE, for example the magnesium dialkyls described in Birkelbach, USP 4,120,820 (Dow). Another group of Ziegler catalysts useful in making polyethylene are those formed by the reaction of organosilols with chromium trioxide, such as described in Baker, USP 3,324,101 (Union Carbide). Ziegler catalysts can be successfully used in suspension, or slurry, systems where the temperature is kept below 110°Cand is run at about 0.5 to 2 MPa to avoid solution in the diluent. In solution polymerization, the system is operated at about 150 - 250°Cand at about 2 - 4 MPa. Gas-phase polymerization, which is run at 70 - 110°C and at 2 - 3 MPa, does not use a hydrocarbon solvent or diluent.
The preparation of polypropylene also involves the use of Ziegler catalysts, which allows the stereo regular polymerization of propylene to form isotactic polypropylene. The catalyst used is typically a titanium trichloride in combination with aluminum
diethylmonochloride, as further described in Cecchin, USP 4,177,160 (incorporated herein). The various types of polymerization processes used for the production of polypropylene include the slurry process, which is run at about 50 - 90°C and 0.5 - 1.5 MPa (5-15 atm), and the gas-phase and liquid-monomer processes, in which extra care must be given to the removal of amorpohous polymer. Functionalized polypropylene, containing functional groups such as maleic anhydride or acrylic acid, is also suitable for use herein.
Various higher olefins can be homopolymerized to form polyolefins using Ziegler-Natta catalysts, among them 1-butene and 4-methyl-1-pentene. 1-Butene is polymerized in solution using an aluminum-reduced TiCl3 catalyst with diethylaluminum chloride as the cocatalyst, as described in Edwards, USP 3,362,940 (incorporated herein). 4-Methyl-1-pentene is prepared by the dimerization of propylene in slurry at about 180°C and 6-7 MPa, as further described in Hashimoto, USP 3,950,450 (incorporated herein).
Component (b)(i) and (e)(i) in the compositions of this invention is an organophosphorous compound, which is employed to increase ignition resistance. Suitable organophosphorous compounds are those which include the organophosphates, the organophosphonites, the organophosphines, the organophosphites and the polyphosphates. Preferred organophosphorus compounds are those containing repeating groups represented by the formulae: or mixtures of and ( I )
Figure imgf000019_0001
Figure imgf000019_0002
or those represented by the formulae:
O = P(OR)3,
R-P-(OR)-OR,
RO-P(OR)-R1-P(OR)-OR,
R-P(R)-OR,
P(R)3, and
P(OR)3
wherein each R is independently a linear or cyclic, substituted or unsubstituted aryl, alkyl, aralkyl, or alkaryl radical containing one to twenty carbon atoms, including halogenated alkyl or aryl radicals, such as methyl, ethyl, isopropyl, cyclopentyl, cyclohexyl, benzyl, tolyl, and/or xylyl; R1 is a 4,4'biphenyl radical; and n is an integer from 1 to 1,000. The preferred
organophosphorous compound is a phosphorous acid ester such as tri phenyl phosphate.
Suitable organophosphorus compositions are disclosed, for example, in U.S. Patent Nos.
4,066,611; 4,073,769; 4,076,686; 4,088,709; 4,427,813; and 4,254,014, each of which is incorporated herein.
Component (b)(ii) and (e)(ii) in the compositions of this invention is fibril -forming poly(tetrafluoroethylene) ("PTFE"). PTFE can be made by the granular polymerization process wherein tetrafluoroethylene ("TFE") is pressured into an agitated aqueous solution of free radical initiator at pressures of 5-80 kg/cm2 and at temperatures of 50-150ºC. Initiators can be redox systems, azo initiators, peroxides or inorganic persulfates. The polymer particles coagulate as they are formed. Fine-powder PTFE can be made by a process similar to the foregoing except that sufficient dispersing agent is used to maintain a stable dispersion throughout polymerization and avoid premature coagulation. The dispersing agent is anionic and substantially non-telogenic, such as a fluorinated carboxylate containing 7-20 carbons. TFE is prepared by reacting hydrogen fluoride and chloroform to give chiorodifluoromethane, which is then pyrolyzed in a noncatalytic gas-phase reaction at atmospheric or reduced pressure, usually at about 590-900°C, to obtain tetrafluoroethylene. The processes for making PTFE described above are discussed in greater detail in U.S. Patents 2,393,967, 3,855,191 and 4,186,121, each of which is incorporated herein.
Fibril-forming PTFE is typically considered to be that which has a structure wherein PTFE particles having an average size of 0.1-0.2 microns are held together by fibrils having diameters from a fourth to a tenth or less of the diameters of the particles. PTFE which loses or does not form such structure, as a result of mechanical shearing, is typically considered to be non-fibril-forming. Fibril-forming PTFE is disclosed, in general, by U.S. Patents 3,005,795, 3,671 ,487 and 4,463,130, each of which is incorporated herein. Most desirably, the PTFE employed in the compositions of this invention has a high elastic memory such that, when incorporated into the polymeric blend and molded into a molded object, such molded object will have a heat shrinkage equal to or greater than 15 percent when tested, for example, at a level of 0.5 weight percent in a composition of this invention in an injection-molded bar measuring 127 mm ×27 mm × 1.6 mm which is heated at 160°Cfor 1 hour. Representative examples of PTFE which have high elastic memory are various members of the Teflon™ PTFE series available from E.I. du Pont de Nemours & Co., to-wit: 6C, 6CN, 60, 64, 65 and 67.
Component (b)(iii) in the compositions of this invention is a dispersing agent. The dispersing agent useful herein may be characterized as a fine, free-flowing powder having an average particle size of less than 1 ,000 microns, advantageously less than 500 microns, preferably, less than 250 microns, more preferably less than 50 microns and most preferably less than 10 micron. Particle size is the greatest dimension of a particle measured in any direction. A free-flowing powder may be further characterized by its ability to flow without
agglomeration when being poured or fed through a narrow opening. Representative examples of such a dispersing agent are ground polycarbonate or an aromatic carbonate oligomer, either of which may be halogenated ornon-halogenated, or other thermoplastic resins such as polyacetal, acrylate and methacrylate polymers and copolymers, polyamide, polyester, ethylene/carbon monoxide copolymer, olefin polymers and copolymers, poly(phenylene ether), polysiloxane, polystyrene, polysulfone, polyurethane, vinyl acetate polymers and copolymers, vinyl alcohol polymers and copolymers, vinyl aromatic copolymers, and vinyl ether polymers and copolymers.
When component (b)(iii) is an aromatic carbonate oligomer, it may be made, in general, by the methods set forth above for the preparation of polycarbonate. As it is aromatic, the carbonyl carbons in the oligomeric chain are bridged by a dihydroxy compound residue some portion of which is an aromatic ring, and as it is an oligomer, it has a degree of polymerization of about 2 to about 30.
When component (b)(iii) is a halogenated carbonate oligomer or polycarbonate, it may be prepared using, for example, an aromatic dihydroxy compound as described by structure above wherein at least one X is halogen. Correspondingly, when it is non-halogenated, it may be made using such an aromatic dihydroxy compound wherein no X is a halogen, and wherein the bridging radical Z is not halogenated. When component (b)(iii) is a halogenated aromatic carbonate oligomer, it may also serve as component (e)(iii).
Representative examples of a suitable halogenated aromatic carbonate oligomer for use as component (e)(iii) is a carbonate oligomer prepared from Tetrabromo Bisphenol-A, which is available from Great Lakes Chemicals as BC-52 or BC-58.
Representative examples of a halogenated aromatic carbonate oligomer suitable for use as the dispersing agent herein or as component (e)(iii) is a carbonate oligomer prepared from Tetrabromo Bisphenol-A, which is available from Great Lakes Chemicals as BC-52 or BC-58.
Component (c) in the compositions of this invention is an elastomeric impact modifier, several different varieties of which, or a mixture thereof, are suitable for use herein. One form which such elastomeric impact modifier may take is a block copolymer which can be either linear, branched, radial or teleblock, and can be either a di-block ("A-B") copolymer, triblock ("A-B-A") copolymer, or radial teleblock copolymer with or without tapered sections, i.e. portions of the polymer where the monomers alternate or are in random order close to the point of transition between the A and B blocks. The A portion is made by polymerizing one or more vinyl aromatic hydrocarbon monomers, and has an average molecular weight of about 4,000 to about 115,000, and a weight preferably of about 8,000 to about 60,000. The B portion of the block copolymer results from polymerizing a diene and has a molecular weight of about 20,000 to about 450,000, and a weight preferably of about 50,000 to about 300,000. In the A-B di-block copolymer, each block, A or B, can vary from 10-90% of the total weight of the copolymer. In the A-B-A tri-block copolymer, the A end groups typically constitute about 2 wt% to about 55 wt% of the whole block copolymer, and preferably are between 5 wt% and 45 wt% of the whole block copolymer.
The A block of the block copolymer has properties characteristic of thermoplastic substances in that it has the stability necessary for processing at elevated temperatures and yet possesses good strength below the temperature at which it softens. The A block is polymerized predominantly from vinyl aromatic hydrocarbons, and substituted derivatives thereof wherein the aromatic moiety can be either mono- or polycyclic. Monomers from which the
thermoplastic end blocks can be formed are, for example, styrene and substituted derivatives thereof such as α-methyl styrene, vinyl xylene, vinyl naphthalene, and the like, and mixtures of two or more thereof. Other vinyl monomers such as methyl acrylate, methyl methacrylate, phenyl maleimide, acrylonitrile or vinyl pyridine may be used in the formation of the A block together with the aromatic monomers. The polymerization can be initiated by lithium metal, or alkyl- or aryl lithium compounds such as butyl lithium or isoamyl lithium. Polymerization is normally conducted at temperatures ranging from about -20ºC to about 100°C. The B block of the copolymer can be formed, for example, simply by injecting suitable monomer into the reaction vessel and displacing the lithium radical from the just-polymerized A block, which then acts as an initiator because it is still charged. The B block is formed predominantly from substituted or unsubstituted C2-C10 dienes, particularly conjugated dienes such as butadiene or isoprene. Other diene, vinyl or olefinic monomers such as chloroprene, 1,4-pentadiene, isobutylene, ethylene or vinyl chloride may be used in the formation of the B block provided that they are present at a level low enough to not alter the fundamental olefinic character of the B block. The B block will be characterized by elastomeric properties which allow it to to absorb and dissipate an applied stress and then regain its shape.
In the A-B-A tri-block copolymer, the second end block A can be formed in a manner similar to the first, by injecting appropriate vinyl aromatic monomer into the reaction vessel. Alternatively, a bivalent lithium initiator can be used, which, when brought together with the diene monomer under the same conditions described above, will form an elastomeric mid block B which carries a charge at each end. Then, upon addition of vinyl aromatic monomer to the reaction mixture, a thermoplastic end block A will form on both ends of the mid block B, yielding a thermoplastic elastomeric A-B-A copolymer.
To reduce oxidative and thermal instability, the block copolymers used herein can also desirably be hydrogenated to reduce the degree of unsaturation on the polymer chain and on the pendant aromatic rings. The block copolymer may be selectively hydrogenated by hydrogenating only the elastomeric block B. Typical hydrogenation catalysts utilized are Raney nickel, molybdenum sulfide, finely divided palladium and platinum oxide. The hydrogenation reaction is typically run at 75-450°F and at 100-1,000 psig for 10-25 hours.
The most preferred vinyl aromatic block copolymers are vinyl
aromatic/conjugated diene block copolymers formed from styrene and butadiene or styrene and isoprene. When the styrene/butadiene copolymers are hydrogenated, they are frequently represented as styrene/(ethylene/butylene) copolymer in the di-block form, or as
styrene/(ethylene/butylene)/styrene copolymer in the tri-block form. When the
styrene/isoprene copolymers are hydrogenated, they are frequently represented as styrene/(ethylene/propylene) copolymer in the di-block form, or as
styrene/(ethylene/propylene)/styrene copolymer in the tri-block form. The vinyl aromatic/diene block copolymers described above are discussed in greater detail in Holden, USP 3,265,766; Haefele, USP 3,333,024; Wald, USP 3,595,942; and Witsiepe, USP 3,651,014, each of which is incorporated herein.
Other elastomeric impact modifiers useful in the compositions of this invention are thermoplastic elastomers, emulsion-type, core-shell graft copolymer elastomers, and olefinic elastomers.
Thermoplastic elastomers are those which are characterized, for example, in that they can be melted and recooled, or dissolved and reformed upon removal of the solvent, without undergoing any significant change in properties. Thermoplastic elastomers are also characterized by the randomness of the shape and size they take on when mixed by shearing forces with the other components making up the compositions of this invention, especially when heat is applied during such mixing. Because thermoplastic elastomer is typically a long chain molecule, segments of a thermoplastic elastomer in the polymer composition matrix are generally elongated, linear ribbons or bands. The molecules tend to fuse and flow together in a continuous structure. However, chain coiling can yield globule-shaped segments of thermoplastic elastomer in the matrix.
The random shape and size assumed in the polymer composition matrix by a thermoplastic elastomer is to be distinguished from the shape and size assumed by a core-shell graft copolymer. A core-shell graft copolymer is typically present in the polymer matrix in a bead shape both before and after mixing by application of shearing forces, whether heat is used or not, and is usually present in a rather narrow size range, for example 0.05-0.8 microns. The retention of this core-shell, or spherical, shape by the graft polymer, even after heating and mixing, results from the fact that the outer layers, which surround the core, are formed by grafting appropriate monomers onto the core. A core-shell graft copolymer typically cannot be melted and recooled without a significant change in properties because the graft polymer will tend to decompose or crosslink, and the bead-shaped segments of graft polymer will tend to agglomerate upon melting, making dispersion of them by mixing difficult.
Thermoplastic elastomers include, for example, an SBR rubber, which is a copolymer of styrene and butadiene typically containing about 23% styrene. The monomers themselves can be randomly dispersed along the backbone, or blocks of each monomer can be randomly dispersed. Thermoplastic elastomers also include the di-block ("A-B") copolymers and the tri-block ("A-B-A") copolymers discussed.
Linear, branched, radial or teleblock A-B-A or A-B block copolymer thermoplastic elastomers can also be prepared from materials other then vinyl aromatic systems. These other copolymers also have a rigid block "A" having a Tg above room temperature (approximately 23-25°C) and a rubbery block "B" having a Tg below room temperature. Examples of typical pairings of the various materials used to form the respective A and B blocks of such other block copolymer thermoplastic elastomers are shown below in Table I.
Figure imgf000024_0001
Block copolymer thermoplastic elastomers can be prepared, for example, by anionic polymerization using an alkyl-lithium initiator. Thermoplastic elastomers based on urethane are discussed in greater detail in Schollenberger, USP 3,015,650 and Saunders, USP 3,214,411 ; and those based on copolyester-ether are discussed in Witsiepe, USP 3,651,014, each of which is incorporated herein.
Representative examples of the core-shell graft copolymer elastomers suitable for use herein are those which can be based on either a diene rubber, an acrylate rubber or on mixtures thereof.
A diene rubber contains a substrate latex, or core, which is made by polymerizing a diene, preferably a conjugated diene, or by copolymerizing a diene with a mono-olefin or polar vinyl compound, such as styrene, acrylonitrile, or an alkyl ester of an unsaturated carboxylic acid such as methyl methacrylate. The substrate latex is typically made up of about 40-85% diene, preferably a conjugated diene, and about 15-60% of the mono-olefin or polar vinyl compound. The elastomeric core phase should have a glass transition temperature ("Tg") of less than about 10°C, and preferably less than about -20°C. A mixture of ethylenicaliy unsaturated monomers is then graft polymerized to the substrate latex. A variety of monomers may be used for this grafting purpose, of which the following are exemplary: vinyl compounds such as vinyl toluene or vinyl chloride; vinyl aromatics such as styrene, alpha-methyl styrene or halogenated styrene; acrylonitrile, methacrylonitrile or alpha-halogenated acrylonitrile; a C1-C8 alkyl acrylate such as ethyl acrylate or hexyl acrylate; a C1-C8 alkyl methacrylate such as methyl methacrylate or hexyl methacrylate; glycidyl methacrylate; acrylic or methacrylic acid; and the like or a mixture of two or more thereof. The preferred grafting monomers include one or more of styrene, acrylonitrile and methyl methacrylate.
The grafting monomers may be added to the reaction mixture simultaneously or in sequence, and, when added in sequence, layers, shells or wart-like appendages can be built up around the substrate latex, or core. The monomers can be added in various ratios to each other although, when just two are used, they are frequently utilized in equal amounts. A typical weight ratio for methyl methacrylate/butadiene/styrene copolymer ("MBS" rubber) is about 60-80 parts by weight substrate latex, about 10-20 parts by weight of each of the first and second monomer shells. A preferred formulation for an MBS rubber is one having a core built up from about 71 parts of butadiene, about 3 parts of styrene, about 4 parts of methyl methacrylate and about 1 part of divinyl benzene; a second phase of about 11 parts of styrene; and a shell phase of about 11 parts of methyl methacrylate and about 0.1 part of 1,3-butylene glycol dimethacrylate, where the parts are by weight of the total composition. A diene-based, core-shell graft copolymer elastomer and methods for making same, as described above, are discussed in greater detail in Saito, USP 3,287,443, Curfman, USP 3,657,391, and Fromuth, USP 4,180,494.
An acrylate rubber has a first phase forming an elastomeric core and a second phase forming a rigid thermoplastic phase about said elastomeric core. The elastomeric core is formed by emulsion or suspension polymerization of monomers which consist of at least about 50 weight percent alkyl and/or aralkyl acrylates having up to fifteen carbon atoms, and, although longer chains may be used, the alkyls are preferably C2-C6, most preferably butyl acrylate. The elastomeric core phase should have a Tg of less than about 10°C, and preferably less than about -20°C.
The rigid thermoplastic phase of the acrylate rubber is formed on the surface of the elastomeric core using suspension or emulsion polymerization techniques. The monomers necessary to create this phase together with necessary initiators are added directly to the reaction mixture in which the elastomeric core is formed, and polymerization proceeds until the supply of monomers is substantially exhausted. Ethylenicaliy unsaturated monomers such as glycidyl methacrylate, or an alkyl ester of an unsaturated carboxylic acid, for example a C1-C8 alkyl acrylate like methyl acrylate, hydroxy ethyl acrylate or hexyl acrylate, or a C1-C8 alkyl methacrylate such as methyl methacrylate or hexyl methacrylate, or mixtures of any of the foregoing, are some of the vinyl monomers which can be used for this purpose. Either thermal or redox initiator systems can be used. Because of the presence of the graft linking agents on the surface of the elastomeric core, a portion of the chains which make up the rigid thermoplastic phase are chemically bonded to the elastomeric core. It is preferred that there be at least about 20% bonding of the rigid thermoplastic phase to the elastomeric core.
A preferred acrylate rubber is made up of more than about 40% to about 95% by weight of an elastomeric core and about 60% to about 5% of a rigid thermoplastic phase. The elastomeric core can be polymerized from about 75% to about 99.8% by weight C1-C6 acrylate, preferably n-butyl acrylate. The rigid thermoplastic phase can be polymerized from at least 50% by weight of C1-C8 alkyl methacrylate, preferably methyl methacrylate. Acrylate rubbers and methods for making same, as described above, are discussed in greater detail in Owens, USP 3,808,180 and Witman, USP 4,299,928.
Olefinic elastomers useful as an impact modifier in the compositions of this invention are based generally on a long-chain, hydrocarbon backbone, which may or may not be grafted with one or more vinyl monomers. Representative examples of a few olefinic elastomers which illustrate the variation in the known substances which would suffice for such purpose are as follows: butyl rubber; chlorinated polyethylene rubber; chlorosulfonated polyethylene rubber; ethylene/propylene copolymer and ethylene/propylene/diene copolymer, which may be grafted with one or more vinyl monomers; neoprene rubber; nitrile rubber; polybutadiene and polyisoprene.
A variety of additives may be used in the compositions of this invention for protection against thermal, oxidative and ultra-violet degradation. Representative of the thermal and oxidative stabilizers which can be advantageously utilized are hindered phenols, hydroquinones, phosphites, including substituted members of those groups and/or mixtures of more than one thereof. A preferred phenolic anti-oxidant is Irganox™ 1076 anti-oxidant, available from Ciba-Geigy Corp. Ultra-violet stabilizers such as various substituted resorcinols, salicylates, benzotriazoles, benzophines, hindered amines and hindered phenols can also be usefully included in the compositions hereof, as can be lubricants, colorants, fillers such as talc, clay, phosphate, metal, inorganic or graphite fibers, or mica, dyes, pigments, mold release agents, and reinforcement agents such as fiberglass or phosphate, metal, inorganic or graphite fibers. Additives and stabilizers of the same or a similar kind as the foregoing are known, and the use and selection thereof is within the skill in the art. However, such additives, if used, typically do not exceed 15 percent by weight of the total composition, except fillers or reinforcing agents, which may constitute up to 40 percent of the composition.
To illustrate the practice of this invention, examples of preferred embodiments
(Examples 1-3) are set forth below. It is notintended, however, that these examples should in any manner restrict the scope of this invention. Some of the particularly desirable features of this invention may be seen by contrasting the characteristics of Examples 1-3 with those of various controlled formulations (Control A-P) which do not possess the features of, and are not therefore embodiments of, this invention.
The formulations of the polycarbonate compositions of Controls A-G and Example 1 are given below in Table II in parts by weight of the total composition. In Table II:
"Polycarbonate" is a polycarbonate having a melt flow rate of 13, as determined according to ASTM Designation D 1238-89, Condition 300/1.2, available from The Dow Chemical Company;
"Polyester" is Tratuf™ 9506 poly(ethylene terephthalate) having an 0.95 intrinsic viscosity, available from Goodyear Tire and Rubber Company; "Paraloid™ 8967" elastomeric copolymer is a methacrylate/butadiene/styrene core-shell elastomer, available from Rohm & Haas Company;
"Phosphate" istriphenyl phosphate, available from Akzo Chemicals, Inc.;
"PTFE" is Teflon™ 6C polymer, fibril-forming poly(tetrafluoroethylene), available from E.I. du Pont de Nemours & Co.;
"BP460" is brominated triphenyl phosphate, available from FMC Corp.;
"TBBA copolymer" is a copolycarbonate prepared from Tetrabromobisphenol-A ("TBBA") and Bisphenol-A ("Bis-A") in a 1/4 TBBA/Bis-A molar ratio;
"Oligocarbonate" is Tetrabromo Bisphenol-A carbonate oligomer, available from Great Lakes Chemical, Inc.; and
"IR 1076" is phenolic anti-oxidant stabilizer, available from Ciba-Geigy
Corporation.
The polycarbonate compositions prepared in Controls A-G and Example 1 are made by dry blending the PTFE and the oligocarbonate in a Lightnin blender to uniformly disperse the PTFE solids in the oligocarbonate. Phosphate and IR 1076 are then added to this batch of predispersed materials. The predispersed materials are then added to a Lightnin blender for mixture with the polycarbonate, the polyester and the Paraloid™ 8967, and this final formulation is mixed for at least 1 minute in the blender with constant agitation of the shaft.
Each dry blended final formulation is then melt mixed in a vented 30mm Werner- Pfleiderer co-rotating, twin screw extruder using a set temperature of 250°C for all barrel zones. Each extruded composition is passed through a water bath, chopped into granules and collected for molding. Granules are thoroughly dried in a circulated air oven at 100°C for at least 4 hours prior to molding. All testing samples are prepared by injection molding on a 55 ton Negri Bossi molding machine, using a 250°C temperature for the barrel.
In Table II, Controls A-G are indicated by Ct-A, Ct-B etc., and Example 1 is indicated by Ex- 1.
Figure imgf000028_0001
Impact resistance is measured on samples of Controls A-G and Example 1 by the Izod test according to ASTM Designation D 256-84 (Method A) at 40°F. The notch is 10 mils (0.254 mm) in radius. Izod results are reported in ft-lb/in. "Percent brittle" indicates the percentage of the samples which broke from impact during the Izod test as opposed to remaining hinged after impact. The surface condition of each sample is evaluated by visual examination, and the condition is reported as "Streaks", which indicates that variations in shading and/or molding flow lines could be observed, or "No Streaks", which indicates that the surface was uniform in appearance.
The U.L (Underwriters Laboratory) 94 burn test is performed on samples of Controls A-G and Example 1 which are 1/16 inch in thickness. A burner is placed under each sample until it ignites, and the time from ignition until burning ceases is measured. It is also noted whether burning causes the sample to drip. The test is repeated 5 times for each sample. The report below indicates total burn time for all 5 samples, how many of the 5 samples dripped, and whether the particular formulation passed the U.L. 94 rating test.
The results of these tests are reported below in Table III. In Table III, Controls A-G are indicated by Ct-A, Ct-B etc., and Example 1 is indicated by Ex-1.
Figure imgf000030_0001
The results of the tests performed on the samples molded from the compositions of Controls A-G and Example 1 demonstrate that the samples in which the PTFE was first blended with a dispersing agent, the oligocarbonate in this case, displayed both a U.L. 94 rating of V-0 at 1/16 inch as well as ductility (as measured by the Izod test) and a non-streaked surface. It should be noted that although Controls E and F both had a V-0 burn rating, they were both also brittle and showed a streaked surface. This indicates that the halogen in the
oligocarbonate dispersing agent is not needed to obtain a desirable level of ignition resistance, but that some means of dispersing the PTFE is needed to obtain good impart and surface properites. It is therefore possible to use a dispersing agent such as a non-halogenated oligocarbonate or ground polycarbonate (or other fine, free-flowing powder) because while the halogen does not diminish the ignition resistance of the composition, the role of the oligocarbonate as a dispersing agent is what is important in these compositions as opposed to any contribution the halogen may make to ignition resistance.
The polycarbonate compositions prepared in Controls H-P and Examples 2 and 3 are made by dry blending the ingredients thereof in a Lightnin blender. The dry blended formulations are then melt mixed in a vented 30mm Werner-Pfleiderer co-rotating, twin screw extruder using a set temperature of 270°C for all barrel zones. Each extruded composition is passed through a water bath, chopped into granules and collected for molding. Granules are thoroughly dried in a circulated air oven at 100°C for at least 4 hours prior to molding. All testing samples are prepared by injection molding on a 55 ton Negri Bossi molding machine, using a 250°C temperature for the barrel.
The formulations of the polycarbonate compositions of Controls H-P and
Examples 2 and 3 are given below in Tables IV and V, in parts by weight of the total composition. In Tables IV and V:
"Polycarbonate" is a polycarbonate having a melt flow rate of 14, as determined according to ASTM Designation D 1238-89, Condition 300/1.2, available from The Dow
Chemical Company;
"Polyester" is Tratuf™ 9506 poly(ethylene terephthalate) having an 0.95 intrinsic viscosity, available from Goodyear Tire and Rubber Company;
"Paraloid™ 8967" elastomeric copolymer is a methacrylate/butadiene/styrene core-shell elastomer, available from Rohm & Haas Company;
"Oligocarbonate" is Tetrabromo Bisphenol-A carbonate oligomer, available from Great Lakes Chemical, Inc.;
"Phosphate" is triphenyl phosphate, available from Akzo Chemicals, Inc.;
"PTFE" is Teflon™ 6C polymer, fibril-forming poly(tetrafluoroethylene), available from E.I. du Pontde Nemours & Co.;
"Quatrex® 6410" resin, is a brominated epoxy novolac oligomer, available from The Dow Chemical Company; and "IR 1076" is phenolic anti-oxidant stabilizer, available from Ciba-Geigy
Corporation.
The U.L. (Underwriters Laboratory) 94 burn test is performed on the samples which are 1/8 and 1/16 inch in thickness. A burner is placed under each sample until it ignites, and the time from ignition until burning ceases is measured. It is also noted whether burning causes the sample to drip. The test is repeated 5 times for each sample, the report below for Controls A-G and Examples 1 and 2 indicates whether the sample passed the U.L.94 rating test.
impact resistance is measured by the Izod test according to ASTM Designation D 256-84 (Method A) at23°C. The notch is 10 mils (0.254 mm) in radius. Izod results are reported in ft-lb/in.
"H.D.T.U.L." is heat deflection temperature underload as measured in accordance with ASTM Designation D 648-82 at 66 psi.
The results of these tests are also reported in Tables IV and V.
In Tables IV and V, Controls H-P are indicated by Ct-H, Ct-J etc., and Examples 2 and 3 are indicated by Ex-2 and Ex-3.
Figure imgf000033_0001
Figure imgf000034_0001
The results of the tests performed on the samples molded from the compositions of Controls H-P and Examples 2 and 3 demonstrate a unique combination of impact, heat and ignition resistance properites, especially in view of the low levels of ignition resistance additives present in these compositions.

Claims

C la ims :
1. A composition of matter comprising, in admixture,
(a) polycarbonate,
(b) one or more members of the group consisting of polyester, an acrylate polymer, a vinyl aromatic copolymer and a polyolefin,
(c) fibril-forming poly(tetrafluoroethylene),
(d) an organophosphorous compound, and
(e) a free-flowing, powdered dispersing agent having an average particle size less than 1 ,000 microns.
2. The composition of Claim 1 further comprising an elastomeric impact modifier.
3. The composition of Claim 1 which does not include an inorganic salt.
4. The composition of Claim 1 in the form of a molded object.
5. The composition of Claim 1 which has a V-0 rating at a thickness of 1/16 inch as determined by the U.L.94 burn test.
6. A method of preparing a blended polycarbonate composition which comprises, in admixture,
(a) polycarbonate,
(b) one or more members of the group consisting of polyester, an acrylate polymer, a vinyl aromatic copolymer and a polyolefin,
(c) fibril-forming poly(tetrafluoroethylene),
(d) an organophosphorous compound, and
(e) a free-flowing, powdered dispersing agent having an average particle size less than 1,000 microns;
said method comprising
(I) first forming a pre-mixture containing component (c), the fibril-forming poly(tetrafluoroethylene), and component (e), the dispersing agent, and
(II) blending components (a), (b) and (d) with said pre-mixture.
7. The method of Claim 6 wherein step II further comprises blending components (a), (b), (d) and an elastomeric impact modifier with said pre-mixture.
8. The method of Claim 6 wherein the composition does not include an inorganic salt.
9. A composition of matter comprising, in admixture, polycarbonate, polyester, fibril-forming poly(tetrafluoroethylene), an organophosphorous compound, and an aromatic halogenated carbonate oligomer.
10. The composition of Claim 9 further comprising an acrylate polymer.
11. The composition of Claim 9 further comprising an elastomeric impact modifier.
12. The composition of Claim 9 wherein the aromatic halogenated carbonate oligomer is present in an amount not exceeding 15 percent of the composition by weight, the organophosphorous compound is present in an amount not exceeding 5 percent of the composition by weight, and the poly(tetrafluoroethylene) is present in an amount not exceeding 5 percent of the composition by weight.
13. The composition of Claim 9 which does not include an inorganic salt.
14. The composition of Claim 9 in the form of a molded object.
15. The composition of Claim 9 which has a V-0 rating at a thickness of 1/16 inch as determined by the U.L.94 burn test.
16. A composition of matter comprising, in admixture, polycarbonate, an acrylate polymer, fibril-forming poly(tetrafluoroethylene), an organophosphorous compound, and an aromatic halogenated carbonate oligomer.
17. The composition of Claim 16 further comprising an elastomeric impact modifier.
18. The composition of Claim 16 wherein the aromatic halogenated carbonate oligomer is present in an amount not exceeding 15 percent of the composition by weight, the organophosphorous compound is present in an amount not exceeding 5 percent of the composition by weight, and the poly(tetrafluoroethylene) is present in an amount not exceeding 5 percent of the composition by weight.
19- The composition of Claim 16 which does not include an inorganic salt.
20. The composition of Claim 16 in the form of a molded object.
21. The composition of Claim 16 which has a V-0 rating at a thickness of 1/16 inch as determined by the U.L.94 burn test.
PCT/US1993/002111 1992-03-10 1993-03-10 Ignition resistant polycarbonate blends WO1993018090A1 (en)