US20040020780A1 - Immersion bias for use in electro-chemical plating system - Google Patents
Immersion bias for use in electro-chemical plating system Download PDFInfo
- Publication number
- US20040020780A1 US20040020780A1 US10/419,717 US41971703A US2004020780A1 US 20040020780 A1 US20040020780 A1 US 20040020780A1 US 41971703 A US41971703 A US 41971703A US 2004020780 A1 US2004020780 A1 US 2004020780A1
- Authority
- US
- United States
- Prior art keywords
- substrate
- electrolyte solution
- anode
- bias
- plating
- Prior art date
- Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
- Abandoned
Abstract
A method for immersing a substrate into a processing solution. The method includes connecting a power supply between a conductive layer on the substrate and an electrode positioned in the processing solution, immersing the substrate into the processing solution, and applying an electrical bias to the conductive layer during the immersion.
Description
- This application is a continuation of co-pending U.S. patent application Ser. No. 09/766,060 filed Jan. 18, 2001, which claims benefit of U.S. Pat. No. 6,258,220, filed Apr. 18, 1999. Each of the aforementioned raelated patent applications are hereby incorporated by reference.
- 1. Field of the Invention
- The present invention generally relates to deposition of a metal film on a substrate. More particularly, the electric current/voltage established between an anode and a substrate seed layer during metal film deposition on a substrate.
- 2. Description of the Related Art
- Electroplating, previously limited in integrated circuit design to the fabrication of lines on circuit boards, is now used to deposit metal film on substrates to form interconnect features, such as vias or trenches. One feature filling method that utilizes electroplating requires initially depositing a diffusion barrier layer on the substrate by a process such as chemical vapor deposition (CVD), physical vapor deposition (PVD), or an electroless plating systems. A seed layer is deposited on the diffusion barrier layer by CVD, PVD, or an electroless plating systems to define a plating surface on the substrate. A metal film is then deposited on the substrate seed layer by electroplating. The deposited metal is planarized by another process such as chemical mechanical polishing (CMP), to define conductive interconnect features.
- Electro-chemical plating (ECP), one embodiment of electroplating, is performed by establishing a voltage across an electrolyte solution between the anode and the substrate seed layer. Both the anode and the substrate seed layer are disposed in contact with the electrolyte solution during ECP. During normal ECP operations, a sufficient negative voltage, known as a plating voltage, is established between the seed layer on the substrate and the anode to attract metal ions in the electrolyte solution to deposit as metal film on the seed layer. The plating voltage is typically applied when the substrate seed layer is fully immersed in the electrolyte solution within the ECP system. A solid-state power supply, applied under the control of a controller, is used to apply electric voltages/currents between the anode and the seed layer. When electroplating substrates, efforts are made to ensure the production of a consistent electric current density across the seed layer on the substrate during the plating process. For each plating location on the seed layer, the metal film deposition rate varies as a function of the electric current density at that location. Therefore, variations in the electric current density across the seed layer on the substrate likely result in inconsistent plating rates and deposited metal film thickness across that seed layer.
- When an ECP system is not being used to deposit metal film on a substrate for an extended period, such as during production downtime, portions of the head assembly such as the electric contacts are typically immersed in the electrolyte solution to limit oxidation of the head assembly that results from exposure of the electric contacts to air. Immersion of the head assembly into the electrolyte solution also minimizes formation of crystals that may form due to evaporation of water from the electrolyte solution containing chemicals such as copper sulfate.
- Typical solid state power supplies for electroplating systems produce a slight or trickle current that flows from the anode to the electric contacts through the electrolyte solution even when the power supply is turned off. This slight or trickle current is known as a current leak, and the extent of the current leak is a quantified value in each solid state power supply. Though the trickle current level is typically small, it can cause metal ions from the electrolyte solution to deposit as metal film on the electric contacts, and thereby alter the electric characteristics of the electric contacts. Changes to the electrical or physical characteristics of the electric contacts, including oxidation, crystal formation, and deposition, adversely affect the consistency of the electric voltage/current supplied by the power supply through the electric contacts via the electrolyte solution to the substrate seed layer and adversely affects the resultant uniformity of the deposition metal film.
- Therefore, there remains a need for an electrochemical plating system that limits the current leakage from the power supply through the electric contacts and reduces the metal film deposition onto the electric contacts resulting from the current leakage.
- The present invention generally provides a method for immersing a substrate into a processing solution. The method includes connecting a power supply between a conductive layer on the substrate and an electrode positioned in the processing solution, immersing the substrate into the processing solution, and applying an electrical bias to the conductive layer during the immersion.
- Embodiments of the invention further provide a method for immersing a substrate into a processing fluid. The method includes electrically connecting a seed layer on the substrate with a first terminal of a power supply, electrically connecting an anode positioned in the electrochemical plating solution to a second terminal of a power supply, immersing the substrate into the electrochemical plating solution, and applying an electrical bias between the first terminal and second terminal during the immersing.
- Embodiments of the invention further provide a method for immersing a semiconductor substrate into an electrochemical plating cell. The method includes securing the substrate to an electrical contact element, rotating the substrate, immersing the substrate into a plating solution contained in the electrochemical plating cell, applying an immersion bias to the substrate during the immersing, and applying a plating bias after the substrate is immersed in the plating solution.
- So that the manner in which the above recited features, advantages and objects of the present invention are attained can be understood in detail, a more particular description of the invention, briefly summarized above, may be had by reference to the embodiments thereof which are illustrated in the appended drawings.
- FIG. 1 is a cross sectional view of one embodiment of electro-chemical plating (ECP) system;
- FIG. 2 is a perspective view of another embodiment of an ECP system;
- FIG. 3 is a top schematic view of the ECP system shown in FIG. 2;
- FIG. 4 is a schematic perspective view of one embodiment of spin-rinse-dry (SRD) module, incorporating rinsing and dissolving fluid inlets;
- FIG. 5 is a side cross sectional view of the SRD module of FIG. 4, and shows a substrate in a processing position vertically disposed between fluid inlets;
- FIG. 6 is a cross sectional view of an embodiment of electroplating process cell;
- FIG. 7 is a partial cross sectional perspective view of an embodiment of a cathode contact ring;
- FIG. 8 is a cross sectional perspective view of the cathode contact ring of
- FIG. 7 showing an alternative embodiment of contact pads;
- FIG. 9 is a cross sectional perspective view of the cathode contact ring of FIG. 7 showing an alternative embodiment of the contact pads and an isolation gasket;
- FIG. 10 is a cross sectional perspective view of the cathode contact ring of FIG. 7 showing an embodiment of the isolation gasket;
- FIG. 11 is a simplified schematic diagram of the electric circuit through each contact;
- FIG. 12 is a cross sectional view of one embodiment of a substrate assembly;
- FIG. 12A is an enlarged cross sectional view of an embodiment of the bladder area of FIG. 12;
- FIG. 13 is a partial cross sectional view of one embodiment of a substrate holder plate;
- FIG. 14 is a partial cross sectional view of one embodiment of a manifold;
- FIG. 15 is a partial cross sectional view of one embodiment of a bladder;
- FIG. 16 is a schematic diagram of one embodiment of an electrolyte solution replenishing system;
- FIG. 17 is a cross sectional view of one embodiment of a rapid thermal anneal (RTA) chamber;
- FIG. 18 is a perspective view of an alternative embodiment of a cathode contact ring;
- FIG. 19 is a partial cross sectional view of an alternative embodiment of seal to be used in a substrate holder assembly;
- FIG. 20 is a cross sectional view of one embodiment of an encapsulated anode that can be used in the process cell shown in FIG. 6;
- FIG. 21 is a cross sectional view of another embodiment of an encapsulated anode that can be used in the process cell shown in FIG. 6;
- FIG. 22 is a cross sectional view of yet another embodiment of an encapsulated anode that can be used in the process cell shown in FIG. 6;
- FIG. 23 is a cross sectional view of another embodiment of an encapsulated anode that can be used in the process cell shown in FIG. 6;
- FIG. 24 is a top schematic view of a mainframe transfer robot having a flipper robot incorporated therein;
- FIG. 25 is an alternative embodiment of the substrate holder system having a rotatable head assembly;
- FIGS. 26a and 26 b are cross sectional views of embodiments of a degasser module;
- FIG. 27 shows a graph of voltage as the ordinate plotted as a function of time plotted as the abscissa for an exemplary metal film deposition process using the substrate holder system shown in FIG. 25; and
- FIG. 28 shows one embodiment of a method that is controlled by the controller of FIG. 3 during immersion of a substrate into electrolyte solution.
- FIG. 29 shows another embodiment of a method that is controlled by the controller of FIG. 3 during immersion of a substrate into electrolyte solution.
- The terms “below”, “above”, “bottom”, “top”, “up”, “down”, “upper”, and “lower” and other positional terms used herein are shown with respect to the embodiments in the figures and may be varied depending on the specific relative orientation of the processing apparatus.
- One aspect of this disclosure relates to multiple embodiments of electro-chemical plating (ECP) systems, all of which are used to deposit a metal film on a seed layer on a substrate. Multiple embodiments of ECP systems are described in detail. A substrate holder system including a head assembly is provided that secures substrates during immersion of substrates into an electrolyte solution within the ECP system. The-head assembly includes electric contacts that controllably supply electricity to the seed layer on the substrate to effect the electric biasing between the anode and the seed layer. Any level of positive voltage biasing of the seed layer relative to the anode can result in metal film deposition on the seed layer. Biasing of the electric contacts relative to the anode when the ECP system is not being used for electroplating is described. The voltage biasing of the electric contacts as described limits the depth of metal film deposition on the electric contacts. Additionally, maintaining the electric contacts immersed in the electrolyte solution during down-time limits chemical crystal formations, with such chemicals as copper sulfate, on the electric contacts. The voltage biasing can also limit metal film deposition of varying depths on the seed layer.
- 1. ECP System and Operation
- The structure and voltage biasing of electric contacts are maintained in a pristine condition against the effects of leakage current in an ECP system. FIG. 1 shows one embodiment of
ECP system 10, such as a fountain plater, used in electroplating. TheECP system 10 includes anelectrolyte cell 12, asubstrate holder system 14, ananode 16, and acontact ring 20. Theelectrolyte cell 12 contains electrolyte solution, and the electrolyte cell has a top opening 21 circumferentially defined by thecontact ring 20. Thesubstrate holder system 14 is disposed above the electrolyte cell and is capable of displacing the substrate to be immersed into and out of the electrolyte solution. The substrate, held by thesubstrate holder system 14, is immersed in and removed from the electrolyte solution through the top opening of the electrolyte cell. Thesubstrate holder system 14 is also capable of securing and positioning the substrate in a desired position within the electrolyte solution during processing. Thecontact ring 20 comprises a plurality of metal or metal alloy electric contacts that electrically contact the substrate seed layer. Acontroller 222 controls the electric voltage/current supplied by a solid-state power supply to the electric contacts. The solid-state power supply is electrically connected to the contacts and to the anode, and the controller provides an electric current to the substrate when the seed layer on the substrate is being plated. Thecontroller 222 thereby determines the electric current/voltage established across the electrolyte solution, from the anode to the seed layer on the substrate. In periods when the seed layer is biased with a positive voltage relative to the anode, metal film can deposit on the seed layer at a rate that is a function of the voltage. A leakage or trickle current is a known current that is provided by any specific solid-state power supply when the power supply is turned off. The following embodiments of ECP system illustrate how the operation of solid-state power supplies can be operated to an ECP system in a manner to limit any metal film deposition or chemical crystal formations that form on the electric contacts as a result of the leakage current. The ECP system overcomes the leakage or trickle current produced by solid-state power supply when the power supply is turned off. - FIG. 2 is a perspective view of one embodiment of
ECP system 200. FIG. 3 is a top schematic view of theECP system 200 of FIG. 2. Referring to both FIGS. 2 and 3, which should be viewed and considered together, theECP system 200 generally comprises aloading station 210, a rapid thermal anneal (RTA)chamber 211, a spin-rinse-dry (SRD)station 212, amainframe 214, and an electrolytesolution replenishing system 220. In one embodiment, theECP system 200 is enclosed in a clean environment using panels such as made from PLEXIGLAS® (a registered trademark of the Rohm and Haas Company of West Philadelphia, Pa.). Themainframe 214 generally comprises amainframe transfer station 216 and a plurality ofprocessing stations 218. Eachprocessing station 218 includes one ormore process cells 240. An electrolytesolution replenishing system 220 is positioned adjacent theECP system 200 and connected to theprocess cells 240 individually to circulate electrolyte solution used for the electroplating process. - The
controller 222, whose components are shown in FIG. 3, comprises a central processing unit (CPU) 260,memory 262,circuit portion 265, input output interface (I/O) 279, and bus, not shown. Thecontroller 222 may be a general-purpose computer, a microprocessor, a microcontroller, or any other known suitable type of computer or controller. TheCPU 260 performs the processing and arithmetic operations for thecontroller 222. Thecontroller 222 controls the processing, robotic operations, timing, and other operations associated with theECP system 200. The controller controls the voltage applied to theanode 16, the seed layer on thesubstrate 22, and the operation of thesubstrate holder assembly 450 as shown in FIG. 6. - The
memory 262 includes random access memory (RAM) and read only memory (ROM) that together store the computer programs, operands, operators, dimensional values, system processing temperatures and configurations, and other parameters that control the electroplating operation. A bus (not numbered) provides for digital information transmissions betweenCPU 260,circuit portion 265,memory 262, and I/O 279. The bus also connects I/O 279 to the portions of theECP system 200 that either receive digital information from, or transmit digital information to, thecontroller 222. - I/
O 279 provides an interface to control the transmissions of digital information between each of the components incontroller 222. I/O 279 also provides an interface between the components of thecontroller 222 and different portions of theECP system 200.Circuit portion 265 comprises all of the other user interface devices, such as display and keyboard. - In this disclosure, the term “substrate” is intended to describe wafers, semiconductor substrates, liquid crystal diode (LCD) displays, or other objects that can be processed within the
ECP system 200. The substrates are generally circular or rectangular, may be of any size, though the circular substrates commonly have a 200 mm or 300 mm diameter, and may include notch or flat edge indentations that assist in providing and maintaining proper wafer orientation about its vertical axis. Theloading station 210 may include one or more substratecassette receiving areas 224, one or more loadingstation transfer robots 228 and at least onesubstrate orientor 230. The number of substrate cassette receiving areas, loadingstation transfer robots 228 and substrate orientors included in theloading station 210 can be configured according to the desired throughput of the system. As shown for one embodiment in FIGS. 2 and 3, theloading station 210 includes two substratecassette receiving areas 224, two loadingstation transfer robots 228 and onesubstrate orientor 230. Asubstrate cassette 232 containing one ormore substrates 234 in vertically-spaced cassette shelves provides a location where the substrates can be stored, removed from, or inserted in conjunction with the ECP system. The loadingstation transfer robot 228transfers substrates 234 between thesubstrate cassette 232 and thesubstrate orientor 230. The loadingstation transfer robot 228 comprises a typical transfer robot commonly known in the art. The substrate orientor 230 positions eachsubstrate 234 in a desired orientation to ensure that the substrate is properly processed. The loadingstation transfer robot 228 also transferssubstrates 234 between theloading station 210 and theSRD station 212 and between theloading station 210 and thethermal anneal chamber 211. - FIG. 4 is a schematic perspective view of a spin-rinse-dry (SRD) module of the present invention, incorporating rinsing and dissolving fluid inlets. FIG. 5 is a side cross sectional view of the SRD module of FIG. 4 and shows a substrate in a processing position vertically disposed between fluid inlets. The
SRD station 212 may include one ormore SRD modules 236 and one or more substrate pass-throughcassettes 238. In one embodiment, theSRD station 212 includes twoSRD modules 236, corresponding to the number of loadingstation transfer robots 228, and a substrate pass-throughcassette 238 is positioned in close proximity to eachSRD module 236. The substrate pass-throughcassette 238 facilitates substrate transfer between theloading station 210 and themainframe 214. The substrate pass-throughcassette 238 provides access to and from both the loadingstation transfer robot 228 and a robot in themainframe transfer station 216. - Referring to FIGS. 4 and 5, the
SRD module 238 comprises a bottom 330 a and asidewall 330 b, and anupper shield 330 c which collectively define aSRD module bowl 330 d, where the shield attaches to the sidewall and assists in retaining the fluids within the SRD module. Alternatively, a removable cover could also be used. Apedestal 336, located in the SRD module, includes apedestal support 332 and apedestal actuator 334. Thepedestal 336 supports thesubstrate 338, shown in FIG. 5, on the pedestal upper surface during processing. Thepedestal actuator 334 rotates the pedestal to spin the substrate and raises and lowers the pedestal during etching, rinsing, and certain spinning of the substrate. The substrate may be held in place on the pedestal by a plurality ofclamps 337. The clamps pivot with centrifugal force and in one embodiment engage the substrate in the edge exclusion zone of the substrate. The clamps engage the substrate only when the substrate lifts off the pedestal during the processing. - The
SRD module 236 is connected between theloading station 210 and themainframe 214. Themainframe 214 generally comprises amainframe transfer station 216 and a plurality ofprocessing stations 218. Referring to FIGS. 2 and 3, themainframe 214, as shown, includes twoprocessing stations 218, eachprocessing station 218 having twoprocess cells 240. Themainframe transfer station 216 includes amainframe transfer robot 242. Themainframe transfer robot 242 may comprise a plurality ofindividual robot arms 244 that provides independent access of substrates in theprocessing stations 218 and theSRD stations 212. As shown in FIG. 3, themainframe transfer robot 242 comprises tworobot arms 244, corresponding to the number ofprocess cells 240 perprocessing station 218. Eachrobot arm 244 includes a robot blade orend effector 2404 for holding a substrate during a substrate transfer. In one embodiment, eachrobot arm 244 may operate independently of the other arm to facilitate independent transfers of substrates in the system. Alternatively, therobot arms 244 operate in a linked fashion such that one robot extends as the other robot arm retracts. - In one embodiment, the
mainframe transfer station 216 includes aflipper robot 248 that facilitates transfer of a substrate from a face-up position on therobot blade 2404 of themainframe transfer robot 242 to a face down position for aprocess cell 240, such as an ECP, that requires face-down processing of substrates. Theflipper robot 248 includes amain body 250 that provides both vertical and rotational movements with respect to a vertical axis of themain body 250 and aflipper robot arm 252 that provides rotational movement along a horizontal axis along theflipper robot arm 252. In one embodiment, avacuum suction gripper 254, disposed at the distal end of theflipper robot arm 252, holds the substrate as the substrate is flipped and transferred by theflipper robot 248. Theflipper robot 248 positions a substrate into theprocess cell 240 for face-down processing. The details of the electroplating process cell will be discussed below. - FIG. 24 is a top schematic view of a mainframe transfer robot incorporating a flipper robot. The
mainframe transfer robot 242 as shown in FIG. 24 serves to transfer substrates between different stations attached the mainframe station, including the processing stations and the SRD stations. Themainframe transfer robot 242 includes a plurality ofrobot arms 2402, two are shown, and aflipper robot 2404 is attached as an end effector for each of therobot arms 2402. Flipper robots are generally known in the art and can be attached as end effectors for substrate handling robots, such as model RR701, available from Rorze Automation, Inc., located in Milpitas, Calif. Themain transfer robot 242 comprising a flipper robot as the end effector is capable of transferring substrates between different stations attached to the mainframe as well as flipping the substrate being transferred to the desired surface orientation, i.e., substrate processing surface being face-down for the electroplating process. In one embodiment, themainframe transfer robot 242 provides independent robot motion along the X-Y-Z axes by therobot arm 2402 and independent substrate flipping rotation by the flipperrobot end effector 2404. By incorporating theflipper robot 2404 as the end effector of the mainframe transfer robot, the substrate transfer process is simplified because the step of passing a substrate from a mainframe transfer robot to a flipper robot is eliminated. - FIG. 6 is a cross sectional view of one embodiment of an
electroplating process cell 400. Theelectroplating process cell 240 shown in FIGS. 2 and 3 may be configured as theelectroplating process cell 400 shown in FIG. 6. Theprocess cell 400 generally comprises ahead assembly 410, aprocess cell 420 and anelectrolyte solution collector 440. In one embodiment, theelectrolyte solution collector 440 is secured onto thebody 442 of themainframe 214 over anopening 443 that defines the location for placement of theprocess cell 420. Theelectrolyte solution collector 440 includes aninner wall 446, anouter wall 448 and a bottom 447 connecting the walls. Anelectrolyte solution outlet 449 is disposed through thebottom 447 of theelectrolyte solution collector 440 and connected to the electrolytesolution replenishing system 220 shown in FIG. 2 through tubes, hoses, pipes or other fluid transfer connectors. - The
head assembly 410 is mounted onto ahead assembly frame 452. Thehead assembly frame 452 includes a mountingpost 454 and acantilever arm 456. The mountingpost 454 is mounted onto thebody 442 of themainframe 214, and thecantilever arm 456 extends laterally from an upper portion of the mountingpost 454. In one embodiment, the mountingpost 454 provides rotational movement with respect to a vertical axis along the mounting post to allow rotation of thehead assembly 410. Thehead assembly 410 is attached to a mountingplate 460 disposed at the distal end of thecantilever arm 456. The lower end of thecantilever arm 456 is connected to acantilever arm actuator 457, such as a pneumatic cylinder, mounted on the mountingpost 454. Thecantilever arm actuator 457 provides pivotal movement of thecantilever arm 456 with respect to the joint between thecantilever arm 456 and the mountingpost 454. When thecantilever arm actuator 457 is retracted, thecantilever arm 456 moves thehead assembly 410 away from theprocess cell 420 to provide the spacing required to remove and/or replace theprocess cell 420 from theelectroplating process cell 400. When thecantilever arm actuator 457 is extended, thecantilever arm 456 moves thehead assembly 410 toward theprocess cell 420 to position the substrate in thehead assembly 410 in a processing position. - The
head assembly 410 generally comprises asubstrate holder assembly 450 and asubstrate assembly actuator 458. Thesubstrate assembly actuator 458 is mounted onto the mountingplate 460, and includes a head assembly shaft 462 extending downwardly through the mountingplate 460. The lower end of the head assembly shaft 462 is connected to thesubstrate holder assembly 450 to position thesubstrate holder assembly 450 in a processing position and in a substrate loading position. - The
substrate holder assembly 450 comprises anelectric contact 466. FIG. 7 is a cross sectional view of one embodiment of aelectric contact 466. In general, theelectric contact 466 comprises an annular body having a plurality of conducting members disposed thereon. The annular body is constructed of an insulating material to electrically isolate the plurality of conducting members. Together the body and conducting members form a diametrically interior substrate seating surface which, during processing, supports a substrate and provides a current thereto. - Referring now to FIG. 7 in detail, one embodiment of
electric contact 466 generally comprises a plurality of conductingmembers 765 at least partially disposed within an annularinsulative body 770. Theinsulative body 770 is shown having aflange 762 and a downwardsloping shoulder portion 764 leading to asubstrate seating surface 768 located below theflange 762. Theflange 762 and thesubstrate seating surface 768 lie in offset and substantially parallel planes. Thus, theflange 762 may be understood to define a first plane while thesubstrate seating surface 768 defines a second plane parallel to the first plane wherein theshoulder 764 is disposed between the two planes. However, electric contact design shown in FIG. 7 is intended to be merely illustrative. In another embodiment, theshoulder portion 764 may be of a steeper angle including a substantially vertical angle so as to be substantially normal to both theflange 762 and thesubstrate seating surface 768. Alternatively, theelectric contact 466 may be substantially planar thereby eliminating theshoulder portion 764. However, for reasons described below, one embodiment comprises theshoulder portion 764 shown in FIG. 6 or some variation thereof. - The conducting
members 765 are defined by a plurality of outerelectric contact pads 780 annularly disposed on theflange 762, a plurality of innerelectric contact pads 772 disposed on a portion of thesubstrate seating surface 768, and a plurality of embedded conductingconnectors 776 which link thepads members 765 are isolated from one another by theinsulative body 770. The insulative body may be made of a plastic such as polyvinylidenefluoride (PVDF), perfluoroalkoxy resin (PFA), TEFLON® (a registered trademark of the E.I. duPont de Nemours and Company) and TEFZEL® (a registered trademark of the E.I. duPont de Nemours and Company) or any other insulating material such as Alumina (Al2O3) or other ceramics. Theouter contact pads 780 are electrically coupled to the power supply to deliver current and voltage to theinner contact pads 772 via theconnectors 776 during processing. In turn, theinner contact pads 772 supply the current and voltage to a substrate by maintaining contact around a peripheral portion of the substrate. Thus, in operation the conductingmembers 765 act as discrete current paths electrically connected to a substrate. - Low resistivity, and conversely high conductivity, are directly related to good plating. To ensure low resistivity, the conducting
members 765 may be made of such exemplary materials as copper (Cu), platinum (Pt), tantalum (Ta), titanium (Ti), gold (Au), silver (Ag), stainless steel or other conducting materials. Low resistivity and low contact resistance may also be achieved by coating the conductingmembers 765 with a conducting material. Thus, the conductingmembers 765 may, for example, be made of copper, that has a resistivity of approximately 2×10−8 Ω·m, coated with platinum that has a resistivity of approximately 10.6×10−8 Ω·m. Coatings such as tantalum nitride (TaN), titanium nitride (TiN), rhodium (Rh), Au, Cu, or Ag on a conductive base materials such as stainless steel, molybdenum (Mo), Cu, and Ti are also possible. Further, since thecontact pads connectors 776, thecontact pads members 765 another, such as stainless steel. Either or both of thepads 772, 180 and conductingconnectors 776 may be coated with a conducting material. Additionally, because plating repeatability may be adversely affected by oxidation that acts as an insulator, theinner contact pads 772 comprise a material resistant to oxidation such as Pt, Ag, or Au. - In addition to being a function of the contact material, the total resistance of each circuit is dependent on the geometry, or shape, of the inner contact
inner contact pads 772 and the force supplied by thecontact ring 466. These factors define a constriction resistance, RCR, at the interface of theinner contact pads 772 and thesubstrate seating surface 768 due to asperities between the two surfaces. Generally, as the applied force is increased the apparent area is also increased. The apparent area is, in turn, inversely related to RCR so that an increase in the apparent area results in a decreased RCR. Thus, to minimize overall resistance it is desired to maximize force. The maximum force applied in operation is limited by the yield strength of a substrate which may be damaged under excessive force and resulting pressure. However, because pressure is related to both force and area, the maximum sustainable force is also dependent on the geometry of theinner contact pads 772. Thus, while thecontact pads 772 may have a flat upper surface as in FIG. 7, other shapes may be used to advantage. For example, two shapes are shown in FIGS. 8 and 9. FIG. 8 shows a knife-edge contact pad and FIG. 9 shows a hemispherical contact pad. A person skilled in the art will readily recognize other shapes which may be used to advantage. A more complete discussion of the relation between contact geometry, force, and resistance is given in Ney Contact Manual, by Kenneth E. Pitney, The J. M. Ney Company, 1973, which is hereby incorporated by reference in its entirety. - The number of
connectors 776 may be varied depending on the particular number of desiredcontact pads 772, shown in FIG. 7. For a 200 mm substrate, at least twenty-fourconnectors 776 are spaced equally over 360° in one embodiment. However, as the number of connectors reaches a critical level, the compliance of the substrate relative to thecontact ring 466 is adversely affected. Therefore, while more than twenty-fourconnectors 776 may be used, contact uniformity may eventually diminish depending on the topography of thecontact pads 772 and the substrate stiffness. Similarly, while less than twenty-fourconnectors 776 may be used, current flow is increasingly restricted and localized, leading to poor plating results. Since the dimensions of the process cell can be configured to suit a particular application. For example, the dimensions would be changed to compensate between a 200 and a 300 mm substrate. - As shown in FIG. 10, the
substrate seating surface 768 comprises anisolation gasket 782. The isolation gasket is disposed on theinsulative body 770 and extends diametrically interior to theinner contact pads 772 to define the inner diameter of thecontact ring 466. Theisolation gasket 782 extends slightly above theinner contact pads 772, e.g., a few mils, and may in one embodiment comprise an elastomer such as VITON® (a registered trademark of the E.I. duPont de Nemours and Company of Wilmington, Del.), TEFLON® (a registered trademark of the E.I. duPont de Nemours and Company of Wilmington, Del.), buna rubber and/or the like. Where theinsulative body 770 also comprises an elastomer theisolation gasket 782 may be of the same material. In the latter embodiment, theisolation gasket 782 and theinsulative body 770 may be monolithic, i.e., formed as a single piece. However, theisolation gasket 782 is formed separate from theinsulative body 770 so that it may be easily removed for replacement or cleaning. - While FIG. 10 shows one embodiment of the
isolation gasket 782 wherein the isolation gasket is seated entirely on theinsulative body 770, FIGS. 8 and 9 show an alternative embodiment. In the latter embodiment, theinsulative body 770 is partially machined away to expose the upper surface of the connectingmember 776 and theisolation gasket 782 is disposed thereon. Thus, theisolation gasket 782 contacts a portion of the connectingmember 776. This design requires less material to be used for theinner contact pads 772 that may be advantageous where material costs are significant such as when theinner contact pads 772 include gold. - During processing, the
isolation gasket 782 maintains contact with a peripheral portion of the substrate plating surface and is compressed to provide a seal between the remainingelectric contact 466 and the substrate. The seal prevents the electrolyte solution from contacting the edge and backside of the substrate. As noted above, maintaining a clean, pristine, contact surface is necessary to achieving high plating repeatability. Previous contact ring designs did not provide consistent plating results because contact surface topography varied over time. The contact ring limits, or substantially minimizes, deposits which would otherwise accumulate on theinner contact pads 772 and change their characteristics thereby producing highly repeatable, consistent, and uniform plating across the substrate plating surface. - FIG. 11 is a simplified schematic diagram representing a possible configuration of the electric circuit for the
contact ring 466. To provide a uniform current distribution between the conductingmembers 765, anexternal resistor 700 is connected in series with each of the conductingmembers 765. The resistance value of theexternal resistor 700, represented as REXT, is greater than the resistance of any other component of the circuit. As shown in FIG. 11, the electric circuit through each conductingmember 765 is represented by the resistance of each of the components connected in series with thepower supply 702. RE represents the resistance of the electrolyte solution, which is typically dependent on the distance between the anode and the cathode contact ring and the chemical composition of the electrolyte solution. Thus, RA represents the resistance of the electrolyte solution adjacent the substrate plating surface 754. RS represents the resistance of the substrate plating surface 754, and RC represents the resistance of thecathode conducting members 765 plus the constriction resistance resulting at the interface between theinner contact pads 772 and the substrate plating layer 754. Generally, the resistance value of the external resistor (REXT) is at least as much as ΣR, where ΣR equals the sum of RE, RA, RS and RC. The resistance value of the external resistor (REXT) is greater than ΣR such that ΣR is negligible and the resistance of each series circuit approximates REXT. - Typically, one power supply is connected to all of the
outer contact pads 780 of theelectric contact 466, resulting in parallel circuits through theinner contact pads 772. However, as the inner contact pad-to-substrate interface resistance varies with eachinner contact pad 772, more current will flow, and thus more plating will occur, at the site of lowest resistance. However, by placing an external resistor in series with each conductingmember 765, the value or quantity of electric current passed through each conductingmember 765 becomes controlled mainly by the value of the external resistor. As a result, the variations in the electrical properties between each of theinner contact pads 772 do not affect the current distribution on the substrate. The uniform current density applied across the plating surface contributes to a uniform plating thickness of the metal film deposited on the seed layer on the substrate. The external resistors also provide a uniform current distribution between different substrates of a process-sequence. - Although the
contact ring 466 is designed to resist deposit buildup on theinner contact pads 772, over multiple substrate plating cycles the substrate-pad interface resistance may increase, eventually reaching an unacceptable value. An electronic sensor/alarm 704 can be connected across theexternal resistor 700 to monitor the voltage/current across the external resistor to address this problem. If the voltage/current across theexternal resistor 700 falls outside of a preset operating range that is indicative of a high substrate-pad resistance, the sensor/alarm 704 triggers corrective measures such as shutting down the plating process until the problems are corrected by an operator. Alternatively, a separate power supply can be connected to each conductingmember 765 and can be separately controlled and monitored to provide a uniform current distribution across the substrate. A very smart system (VSS) may also be used to modulate the current flow. The VSS typically comprises a processing unit and any combination of devices known in the industry used to supply and/or control current such as variable resistors, separate power supplies, etc. As the physiochemical, and hence electrical, properties of theinner contact pads 772 change over time, the VSS processes and analyzes data feedback. The data is compared to pre-established setpoints and the VSS then makes appropriate current and voltage alterations to ensure uniform deposition. - FIG. 18 is a perspective view of an alternative embodiment of a cathode contact ring. The
cathode contact ring 1800 as shown in FIG. 18 comprises a conductive metal or a metal alloy, such as stainless steel, copper, silver, gold, platinum, titanium, tantalum, and other conductive materials, or a combination of conductive materials, such as stainless steel coated with platinum. Thecathode contact ring 1800 includes anupper mounting portion 1810 adapted for mounting the cathode contact ring onto the substrate holder assembly and a lowersubstrate receiving portion 1820 adapted for receiving a substrate therein. Thesubstrate receiving portion 1820 includes an annularsubstrate seating surface 1822 having a plurality of contact pads orbumps 1824 disposed thereon and evenly spaced apart. When a substrate is positioned on thesubstrate seating surface 1822, thecontact pads 1824 physically contact a peripheral region of the substrate to provide electric contact to the electroplating seed layer on the substrate deposition surface. Thecontact pads 1824 are coated with a noble metal, such as platinum or gold, that is resistant to oxidation. - The exposed surfaces of the cathode contact ring, except the surfaces of the contact pads that come in contact with the substrate, are treated to provide hydrophilic surfaces or coated with a material that exhibits hydrophilic properties. Hydrophilic materials and hydrophilic surface treatments are known in the art. One company providing a hydrophilic surface treatment is Millipore Corporation, located in Bedford, Mass. The hydrophilic surface significantly reduces beading of the electrolyte solution on the surfaces of the cathode contact ring and promotes smooth dripping of the electrolyte solution from the cathode contact ring after the cathode contact ring is removed from the electroplating bath or electrolyte solution. By providing hydrophilic surfaces on the cathode contact ring that facilitate run-off of the electrolyte solution, plating defects caused by residual electrolyte solution on the cathode contact ring are significantly reduced. The inventors also contemplate application of this hydrophilic treatment or coating in other embodiments of cathode contact rings to reduce residual electrolyte solution beading on the cathode contact ring and the plating defects on a subsequently processed substrate that may result therefrom.
- Referring to FIGS. 12 and 12A, the
substrate holder assembly 464 is positioned above theelectric contact 466 and comprises a bladder assembly 470 that provides pressure to the backside of a substrate and ensures electric contact between the substrate plating surface and theelectric contact 466. The inflatable bladder assembly 470 is disposed on asubstrate holder plate 832. Abladder 836 disposed on a lower surface of thesubstrate holder plate 832 is thus located opposite and adjacent to the contacts on theelectric contact 466 with thesubstrate 821 interposed therebetween. Afluid source 838 supplies a fluid, i.e., a gas or liquid, to thebladder 836 allowing thebladder 836 to be inflated to varying degrees. - Referring now to FIGS. 12, 12A, and13, the details of the bladder assembly 470 will be discussed. The
substrate holder plate 832 is shown as substantially disc-shaped having anannular recess 840 formed on a lower surface and a centrally disposedvacuum port 841. One ormore inlets 842 are formed in thesubstrate holder plate 832 and lead into the relatively enlargedannular mounting channel 843 and theannular recess 840. Quick-disconnect hoses 844 couple thefluid source 838 to theinlets 842 to provide a fluid thereto. Thevacuum port 841 is attached to a vacuum/pressure pumping system 859 adapted to selectively supply a pressure or create a vacuum at a backside of thesubstrate 821. The pumping system 859, shown in FIG. 12, comprises a pump 845, across-over valve 847, and avacuum ejector 849 commonly known as a venturi. One vacuum ejector that may be used is available from SMC Pneumatics, Inc., of Indianapolis, Ind. The pump 845 may be a commercially available compressed gas source and is coupled to one end of a hose 851, the other end of the hose 851 being coupled to thevacuum port 841. The hose 851 is split into apressure line 853 and avacuum line 855 having thevacuum ejector 849 disposed therein. Fluid flow is controlled by thecross-over valve 847 which selectively switches communication with the pump 845 between thepressure line 853 and thevacuum line 855. The cross-over valve has an OFF setting whereby fluid is restricted from flowing in either direction through hose 851. A shut-offvalve 861 disposed in hose 851 prevents fluid from flowing frompressure line 855 upstream through thevacuum ejector 849. The desired direction of fluid flow is indicated by arrows. - Where the
fluid source 838 is a gas supply it may be coupled to hose 851 thereby eliminating the need for a separate compressed gas supply, i.e., pump 845. Further, a separate gas supply and vacuum pump may supply the backside pressure and vacuum conditions. While one embodiment allows for both a backside pressure as well as a backside vacuum, a simplified embodiment may comprise a pump capable of supplying only a backside vacuum. However, as will be explained below, deposition uniformity may be improved where a backside pressure is provided during processing. Therefore, a vacuum ejector and a cross-over valve may be included. - Referring now to FIGS. 12A and 14, a substantially circular ring-shaped
manifold 846 is disposed in theannular recess 840. The manifold 846 comprises a mountingrail 852 disposed between aninner shoulder 848 and anouter shoulder 850. The mountingrail 852 is adapted to be at least partially inserted into theannular mounting channel 843. A plurality offluid outlets 854 formed in the manifold 846 provide communication between theinlets 842 and thebladder 836.Seals 837, such as O-rings, are disposed in theannular manifold channel 843 in alignment with theinlet 842 andoutlet 854 and secured by thesubstrate holder plate 832 to ensure an airtight seal. Conventional fasteners such as screws may be used to secure the manifold 846 to thesubstrate holder plate 832 via cooperating threaded bores formed in the manifold 846 and thesubstrate holder plate 832. - Referring now to FIG. 15, the
bladder 836 is shown, in section, as an elongated substantially semi-tubular piece of material having annular lip seals 856, or nodules, at each edge. In FIG. 12A, the lip seals 856 are shown disposed on theinner shoulder 848 and theouter shoulder 850. A portion of thebladder 836 is compressed against the walls of theannular recess 840 by the manifold 846 which has a width slightly less, e.g., a few millimeters, than theannular recess 840. Thus, the manifold 846, thebladder 836, and theannular recess 840 cooperate to form a fluid-tight seal. To prevent fluid loss, thebladder 836 includes (is formed entirely from or is coated with) some fluid impervious material such as silicon rubber or any comparable elastomer which is chemically inert with respect to the electrolyte solution and exhibits reliable elasticity. Where needed a compliant covering 857 may be disposed over thebladder 836, as shown in FIG. 15, and secured by means of an adhesive or thermal bonding. The covering 857 preferably comprises an elastomer such as VITON®, buna rubber or the like, which may be reinforced by KEVLAR® (a registered trademark of the E.I. duPont de Nemours and Company of Wilmington, Del.), for example. In one embodiment, the covering 857 and thebladder 836 comprise the same material. The covering 857 has particular application where thebladder 836 is liable to rupturing. Alternatively, thebladder 836 thickness may simply be increased during its manufacturing to reduce the likelihood of puncture. The exposed surface of thebladder 836, if uncovered, and the exposed surface of the covering 857 my be coated or treated to provide a hydrophilic surface. This coating promotes dripping and removal of the residual electrolyte solution after the head assembly is lifted above the process cell. - The precise number of
inlets 842 andoutlets 854 may be varied according to the particular application. For example, while FIG. 12 shows two inlets with corresponding outlets, an alternative embodiment could employ a single fluid inlet that supplies fluid to thebladder 836. - In operation, the
substrate 821 is introduced into the container body 802 by securing it to the lower side of thesubstrate holder plate 832. This is accomplished by engaging the pumping system 159 to evacuate the space between thesubstrate 821 and thesubstrate holder plate 832 viaport 841 thereby creating a vacuum condition. Thebladder 836 is then inflated by supplying a fluid such as air or water from thefluid source 838 to theinlets 842. The fluid is delivered into thebladder 836 via themanifold outlets 854, thereby pressing thesubstrate 821 uniformly against the contacts of theelectric contact 466. The electroplating process is then carried out. Electrolyte solution is then pumped into theprocess cell 420 toward thesubstrate 821 to contact the exposedsubstrate plating surface 820. The power supply provides a negative bias to thesubstrate plating surface 820 via theelectric contact 466. As the electrolyte solution is flowed across thesubstrate plating surface 820, ions in the electrolytic solution are attracted to thesurface 820 and deposit on thesurface 820 to form the desired film. - Because of its flexibility, the
bladder 836 deforms to accommodate the asperities of the substrate backside and contacts of theelectric contact 466 thereby mitigating misalignment with the conductingelectric contact 466. Thecompliant bladder 836 prevents the electrolyte solution from contaminating the backside of thesubstrate 821 by establishing a fluid tight seal at a portion close to the perimeter of a backside of thesubstrate 821. Once inflated, a uniform pressure is delivered downward toward theelectric contact 466 to achieve substantially equal force at all points where thesubstrate 821 andelectric contact 466 interface. The force can be varied as a function of the pressure supplied by thefluid source 838. Further, the effectiveness of the bladder assembly 470 is not dependent on the configuration of theelectric contact 466. For example, while FIG. 12 shows a pin configuration having a plurality of discrete contact points, theelectric contact 466 may also be a continuous surface. - Because the force delivered to the
substrate 821 by thebladder 836 is variable, adjustments can be made to the current flow supplied by thecontact ring 466. As described above, an oxide layer may form on theelectric contact 466 and act to restrict current flow. However, increasing the pressure of thebladder 836 may counteract the current flow restriction due to oxidation. As the pressure is increased, the malleable oxide layer is compromised and superior contact between theelectric contact 466 and thesubstrate 821 results. The effectiveness of thebladder 836 in this capacity may be further improved by altering the geometry of theelectric contact 466. For example, a knife-edge geometry is likely to penetrate the oxide layer more easily than a dull rounded edge or flat edge. - Additionally, the fluid tight seal provided by the
inflated bladder 836 allows the pump 845 to maintain a backside vacuum or pressure either selectively or continuously, before, during, and after processing. Generally, however, the pump 845 is run to maintain a vacuum only during the transfer of substrates to and from theelectroplating process cell 400 because it has been found that thebladder 836 is capable of maintaining the backside vacuum condition during processing without continuous pumping. Thus, while inflating thebladder 836, as described above, the backside vacuum condition is simultaneously relieved by disengaging the pumping system 859, e.g., by selecting an off position on thecross-over valve 847. Disengaging the pumping system 859 may be abrupt or comprise a gradual process whereby the vacuum condition is ramped down. Ramping allows for a controlled exchange between the inflatingbladder 836 and the simultaneously decreasing backside vacuum condition. This exchange may be controlled manually or by computer. - As described above, continuous backside vacuum pumping while the
bladder 836 is inflated is not needed and may actually cause thesubstrate 820 to buckle or warp leading to undesirable deposition results. It may be desirable to provide a backside pressure to thesubstrate 820 in order to cause a “bowing” effect of the substrate to be processed. Bowing of the substrate may results in superior deposition on the substrate since portions, such as the periphery, of the substrate are displaced by the bowing nearer to the anode than other portions. The bowing may make the metal film deposition more uniform if portions of the seed layer having a lesser current density are displaced closer to the anode to make the electric current density more uniform across the substrate. Thus, pumping system 859 is capable of selectively providing a vacuum or pressure condition to the substrate backside. For a 200 mm substrate, for example, a backside pressure up to 5 psi is selected to bow the substrate. The degree of bowing is variable according to the pressure supplied by pumping system 859. Because substrates typically exhibit some measure of pliability, a backside pressure causes the substrate to bow or assume a convex shape relative to the upward flow of the electrolyte solution. - Those skilled in the art will readily recognize other embodiments. For example, while FIG. 12A shows a
bladder 836 having a surface area sufficient to cover a relatively small perimeter portion of the substrate backside at a diameter substantially equal to theelectric contact 466. The geometric configuration of the bladder assembly 470 can be varied. Thus, the bladder assembly may be constructed using more fluid impervious material to cover an increased surface area of thesubstrate 821. - FIG. 19 is a partial cross sectional view of an alternative embodiment of a substrate holder assembly. The alternative
substrate holder assembly 1900 comprises a bladder assembly 470, as described above, having theinflatable bladder 836 attached to the back surface of an intermediarysubstrate holder plate 1910. A portion of theinflatable bladder 836 is sealingly attached to theback surface 1912 of the intermediarysubstrate holder plate 1910 using an adhesive or other bonding material. The front surface 1914 of the intermediarysubstrate holder plate 1910 is adapted to receive asubstrate 821 to be processed. An elastomeric o-ring 1916 is disposed in anannular groove 1918 on the front surface 1914 of the intermediarysubstrate holder plate 1910 to contact a peripheral portion of the substrate back surface. The elastomeric o-ring 1916 provides a seal between the substrate back surface and the front surface of the intermediary substrate holder plate. The intermediary substrate holder plate includes a plurality of bores orholes 1920 extending through the plate that are in fluid communication with thevacuum port 841. The plurality ofholds 1920 facilitate securing the substrate on the substrate holder plate using a vacuum force applied to the backside of the substrate. According to this alternative embodiment of the substrate holder assembly, the inflatable bladder does not directly contact a substrate being processed, and thus the risk of cutting or damaging the inflatable bladder during substrate transfers is significantly reduced. The elastomeric O-ring 1916 may be coated or treated to provide a hydrophilic surface for contacting the substrate. The elastomeric O-ring 1916 is replaced as needed to ensure proper contact and seal to the substrate. - FIG. 25 is an alternative embodiment of the
substrate holder system 14 having arotatable head assembly 2410. In one embodiment, a rotational actuator is disposed on the cantilevered arm and attached to the head assembly to rotate the head assembly during substrate processing. Therotatable head assembly 2410 is mounted onto ahead assembly frame 2452. The alternative embodiment ofhead assembly frame 2452 and therotatable head assembly 2410 are mounted onto the mainframe similarly to thehead assembly frame 452 andhead assembly 410 as shown in FIG. 6 and described above. Thehead assembly frame 2452 includes a mountingpost 2454, apost cover 2455, and acantilever arm 2456. The mountingpost 2454 is mounted onto the body of themainframe 214, and thepost cover 2455 covers a top portion of the mountingpost 2454. In one embodiment, the mountingpost 454 provides rotational movement, as indicated by arrow A1, with respect to a vertical axis along the mounting post to allow rotation of thehead assembly frame 2452. Thecantilever arm 2456 extends laterally from an upper portion of the mountingpost 2454 and is pivotally connected to thepost cover 2455 at the pivot joint 2459. Therotatable head assembly 2410 is attached to a mountingslide 2460 disposed at the distal end of thecantilever arm 2456. The mountingslide 2460 guides the vertical motion of thehead assembly 2410. Ahead lift actuator 2458 is disposed on top of the mountingslide 2460 to provide vertical displacement of thehead assembly 2410. - The lower end of the
cantilever arm 2456 is connected to theshaft 2453 of acantilever arm actuator 2457, such as a pneumatic cylinder or a lead-screw actuator, mounted on the mountingpost 2454. Thecantilever arm actuator 2457 provides pivotal movement, as indicated by arrow A2, of thecantilever arm 2456 with respect to the pivot joint 2459 between thecantilever arm 2456 and thepost cover 2454. When thecantilever arm actuator 2457 is retracted, thecantilever arm 2456 moves thehead assembly 2410 away from theprocess cell 420. The movement of thehead assembly 2410 provide the spacing required to remove and/or replace theprocess cell 420 from theelectroplating process cell 240. When thecantilever arm actuator 2457 is extended, thecantilever arm 2456 moves thehead assembly 2410 toward theprocess cell 420 to position the substrate in thehead assembly 2410 in a processing position. - The
rotatable head assembly 2410 includes arotating actuator 2464 slideably connected to the mountingslide 2460. Theshaft 2468 of thehead lift actuator 2458 is inserted through alift guide 2466 attached to the body of therotating actuator 2464. In an embodiment, theshaft 2468 is a lead-screw type shaft that moves the lift guide, as indicated by arrows A3, between various vertical positions. Therotating actuator 2464 is connected to thesubstrate holder assembly 2450 through theshaft 2470 and rotates thesubstrate holder assembly 2450, as indicated by arrows A4. Thesubstrate holder assembly 2450 includes a bladder assembly, such as the embodiments described above with respect to FIGS. 12-15 and 19, and a cathode contact ring, such as the embodiments described above with respect to FIGS. 7-10 and 18. - The rotation of the substrate during the electroplating process generally enhances the deposition results. In one embodiment, the head assembly is rotated between about 2 rpm and about 200 rpm, preferably between about 20 and 40 rpm, when the substrate is immersed in the electrolyte solution, during the electroplating process. The
substrate holder assembly 2472 can be rotated to impart rotation to the substrate as thesubstrate holder system 14 lowers the seed layer on the substrate into contact with the electrolyte solution in the process cell. The head assembly is raised to remove the seed layer on the substrate from the electrolyte solution in the process cell. The head assembly is preferably rotated at a high speed, i.e., between about 100 and 2500 rpm, after the head assembly is lifted from the process cell to enhance removal of residual electrolyte solution from the head assembly by centrifugel force. - In one embodiment, the uniformity of the deposited film has been improved within about 2%, i.e., maximum deviation of deposited film thickness is at about 2% of the average film thickness, while standard electroplating processes typically achieves uniformity at best within about 5.5%. However, rotation of the head assembly is not necessary to achieve uniform electroplating deposition in some instances, particularly where the uniformity of electroplating deposition is achieved by adjusting the processing parameters, such as the chemicals in the electrolyte solution, electrolyte solution flow and other parameters.
- Referring back to FIG. 6, a cross sectional view of an
electroplating process cell 400, thesubstrate holder assembly 450 is positioned above theprocess cell 420. Theprocess cell 420 generally comprises abowl 430, acontainer body 472, ananode assembly 474 and afilter 476. In one embodiment, theanode assembly 474 is disposed below thecontainer body 472 and attached to a lower portion of thecontainer body 472, and thefilter 476 is disposed between theanode assembly 474 and thecontainer body 472. Thecontainer body 472 is preferably a cylindrical body comprised of an electrically insulative material, such as ceramics, plastics, PLEXIGLAS® (acrylic), lexane, PVC, CPVC, and PVDF. Alternatively, thecontainer body 472 can be made from a coated metal, such as stainless steel, nickel and titanium. The coated metal is coated with an insulating layer such as TEFLON® (a trademark of the E. I. duPont de Nemoirs Company of Wilmington, Del.), PVDF, plastic, rubber and other combinations of materials that do not dissolve in the electrolyte solution. The insulating layer can be electrically insulated from the electrodes, i.e., the anode and cathode of the ECP system. Thecontainer body 472 is sized and adapted to conform to the substrate plating surface and the shape of the of a substrate being processed through the system, typically circular or rectangular in shape. One embodiment of thecontainer body 472 comprises a cylindrical ceramic tube having an inner diameter that has about the same dimension as or slightly larger than the substrate diameter. Rotational movement typically required in typical ECP systems is not required to achieve uniform plating results when the size of the container body conforms to about the size of the substrate plating surface. - An upper portion of the
container body 472 extends radially outwardly to form anannular weir 478. Theweir 478 extends over theinner wall 446 of theelectrolyte solution collector 440 and allows the electrolyte solution to flow into theelectrolyte solution collector 440. The upper surface of theweir 478 matches the lower surface of theelectric contact 466. The upper surface of theweir 478 includes an inner annularflat portion 480, a middleinclined portion 482 and an outer declinedportion 484. When a substrate is positioned in the processing position, the substrate plating surface is positioned above the cylindrical opening of thecontainer body 472. A gap for electrolyte solution flow is formed between the lower surface of theelectric contact 466 and the upper surface of theweir 478. The lower surface of theelectric contact 466 is disposed above the innerflat portion 480 and the middle inclined portion of theweir 478. The outer declinedportion 484 is sloped downwardly to facilitate flow of the electrolyte solution into theelectrolyte solution collector 440. - A lower portion of the
container body 472 extends radially outwardly to form a lowerannular flange 486 for securing thecontainer body 472 to thebowl 430. The outer dimension, i.e., circumference, of theannular flange 486 is smaller than the dimensions of theopening 444 and the inner circumference of theelectrolyte solution collector 440. The smaller dimension of the annular flange to allow removal and replacement of theprocess cell 420 from theelectroplating process cell 400. In one embodiment,multiple bolts 488 are fixedly disposed on theannular flange 486 and extend downwardly through matching bolt holes on thebowl 430. A plurality ofremovable fastener nuts 490 secure theprocess cell 420 onto thebowl 430. Aseal 487, such as an elastomer O-ring, is disposed betweencontainer body 472 and thebowl 430 radially inwardly from thebolts 488 to prevent leaks from theprocess cell 420. The nuts/bolts combination facilitates fast and easy removal and replacement of the components of theprocess cell 420 during maintenance. - In one embodiment, the
filter 476 is attached to and completely covers the lower opening of thecontainer body 472, and theanode assembly 474 is disposed below thefilter 476. A spacer 492 is disposed between thefilter 476 and theanode assembly 474. In an embodiment, thefilter 476, the spacer 492, and theanode assembly 474 are fastened to a lower surface of thecontainer body 472 using removable fasteners, such as screws and/or bolts. Alternatively, thefilter 476, the spacer 492, and theanode assembly 474 are removably secured to thebowl 430. - The
anode assembly 474 in one embodiment comprises a consumable anode that serves as a metal source in the electrolyte solution. Alternatively, theanode assembly 474 comprises a non-consumable anode, and the metal to be electroplated is supplied within the electrolyte solution from the electrolytesolution replenishing system 220. As shown in FIG. 6, theanode assembly 474 is a self-enclosed module having a porous anode enclosure 494 that may be made of the same metal as the metal to be electroplated, such as copper. Alternatively, the anode enclosure 494 is made of porous materials, such as ceramics or polymeric membranes. A soluble metal 496, such as high purity copper for electro-chemical plating of copper, is disposed within the anode enclosure 494. The soluble metal 496 preferably comprises metal particles, wires or a perforated sheet. The porous anode enclosure 494 also acts as a filter that keeps the particulates generated by the dissolving metal within the anode enclosure 494. As compared to a non-consumable anode, the consumable, i.e., soluble, anode provides gas-generation-free electrolyte solution and minimizes the need to constantly replenish the metal in the electrolyte solution. - An
anode electrode contact 498 is inserted through the anode enclosure 494 to provide electrical connection to the soluble metal 496 from a power supply. In one embodiment, theanode electrode contact 498 is made from a conductive material that is insoluble in the electrolyte solution, such as titanium, platinum and platinum-coated stainless steel. Theanode electrode contact 498 extends through thebowl 430 and is connected to an electric power supply. Preferably, the anodeelectric contact 498 includes a threadedportion 497 for afastener nut 499 to secure the anodeelectric contact 498 to thebowl 430, and aseal 495 such as a elastomer washer, is disposed between thefastener nut 499 and thebowl 430 to prevent leaks from theprocess cell 420. - The
bowl 430 generally comprises acylindrical portion 502 and abottom portion 504. An upperannular flange 506 extends radially outwardly from the top of thecylindrical portion 502. The upperannular flange 506 includes a plurality ofholes 508 that matches the number ofbolts 488 from the lowerannular flange 486 of thecontainer body 472.Bolts 488 are inserted through theholes 508, and thefastener nuts 490 are fastened onto thebolts 488 that secure the upperannular flange 506 of thebowl 430 to the lowerannular flange 486 of thecontainer body 472. In one embodiment, the outer dimension, i.e., circumference, of the upperannular flange 506 is about the same as the outer dimension, i.e., circumference, of the lowerannular flange 486. Preferably, the lower surface of the upperannular flange 506 of thebowl 430 rests on a support flange of themainframe 214 when theprocess cell 420 is positioned on themainframe 214. - The inner circumference of the
cylindrical portion 502 accommodates theanode assembly 474 and thefilter 476. Preferably, the outer dimensions of thefilter 476 and theanode assembly 474 are slightly smaller than the inner dimension of thecylindrical portion 502. These relative dimensions force a substantial portion of the electrolyte solution to flow through theanode assembly 474 first before flowing through thefilter 476. Thebottom portion 504 of thebowl 430 includes anelectrolyte solution inlet 510 that connects to an electrolyte solution supply line from the electrolytesolution replenishing system 220. In one embodiment, theanode assembly 474 is disposed about a middle portion of thecylindrical portion 502 of thebowl 430. Theanode assembly 474 is configured to provide a gap for electrolyte solution flow between theanode assembly 474 and theelectrolyte solution inlet 510 on thebottom portion 504. - The
electrolyte solution inlet 510 and the electrolyte solution supply line are connected by a releasable connector that facilitates easy removal and replacement of theprocess cell 420. When theprocess cell 420 needs maintenance, the electrolyte solution is drained from theprocess cell 420, and the electrolyte solution flow in the electrolyte solution supply line is discontinued and drained. The connector for the electrolyte solution supply line is released from theelectrolyte solution inlet 510, and the electric connection to theanode assembly 474 is also disconnected. Thehead assembly 410 is raised or rotated to provide clearance for removal of theprocess cell 420. Theprocess cell 420 is then removed from themainframe 214, and a new or reconditioned process cell is replaced into themainframe 214. - Alternatively, the
bowl 430 can be secured onto the support flange of themainframe 214, and thecontainer body 472 along with the anode and the filter are removed for maintenance. In this case, the nuts securing theanode assembly 474 and thecontainer body 472 to thebowl 430 are removed to facilitate removal of theanode assembly 474 and thecontainer body 472. New or reconditionedanode assembly 474 andcontainer body 472 are then replaced into themainframe 214 and secured to thebowl 430. - FIG. 20 is a cross sectional view of one embodiment of an encapsulated anode. The encapsulated
anode 2000 includes a permeable anode enclosure that filters or traps “anode sludge” or particulates generated as the metal is dissolved from theanode plate 2004. As shown in FIG. 20, theanode plate 2004 comprises a solid piece of copper. In one embodiment, theanode plate 2004 is a high purity, oxygen free copper, enclosed in a hydrophilicanode encapsulation membrane 2002. Theanode plate 2004 is secured and supported by a plurality of electric contacts or feed-throughs 2006 that extend through the bottom of thebowl 430. The electric contacts or feed-throughs 2006 extend through theanode encapsulation membrane 2002 into the bottom surface of theanode plate 2004. The flow of the electrolyte solution, as indicated by the arrow A, from theelectrolyte solution inlet 510 disposed at the bottom of thebowl 430 through the gap between the anode and the bowl sidewall. The electrolyte solution also flows through theanode encapsulation membrane 2002 by permeation into and out of the gap between the anode encapsulation membrane and the anode plate, as indicated by the arrow B. In one embodiment, theanode encapsulation membrane 2002 comprises a hydrophilic porous membrane, such as a modified polyvinyllidene fluoride membrane, having porosity between about 60% and 80%, more preferably about 70%, and pore sizes between about 0.025 μm and about 1 μm, more preferably between about 0.1 μm and about 0.2 μm. One example of a hydrophilic porous membrane is the Durapore Hydrophilic Membrane, available from Millipore Corporation, located in Bedford, Mass. As the electrolyte solution flows through the encapsulation membrane, anode sludge and particulates generated by the dissolving anode are filtered or trapped by the encapsulation membrane. Thus, the encapsulation membranes improve the purity of the electrolyte solution during the electroplating process, and defect formations on the substrate during the electroplating process caused by anode sludge and contaminant particulates are significantly reduced. - FIG. 21 is a cross sectional view of another embodiment of an encapsulated anode. The
anode plate 2004 is secured and supported on the electric feed-throughs 2006. Atop encapsulation membrane 2008 and abottom encapsulation membrane 2010, disposed respectively above and below theanode plate 2004, are attached to amembrane support ring 2012 that is disposed around theanode plate 2004. The top andbottom encapsulation membranes membrane support ring 2012 comprises a relatively rigid material as compared to the encapsulation membrane, such as plastic or other polymers. Abypass fluid inlet 2014 is disposed through the bottom of thebowl 430 and through thebottom encapsulation membrane 2010 to introduce electrolyte solution into the gap between the encapsulation membranes and the anode plate. Abypass outlet 2016 is connected to themembrane support ring 2012 and extends through thebowl 430 to facilitate flow of excess electrolyte solution with the anode sludge or generated particulates out of the encapsulated anode into a waste drain, not shown. - In one embodiment, the flow of the electrolyte solution within the
bypass fluid inlet 2014 and the mainelectrolyte solution inlet 510 are individually controlled byflow control valves flow control valves bypass fluid inlet 2014 is maintained at a higher pressure than the pressure in the mainelectrolyte solution inlet 510. The flow of the electrolyte solution inside thebowl 430 from the mainelectrolyte solution inlet 510 is indicated by arrows A, and the flow of the electrolyte solution inside the encapsulatedanode 2000 is indicated by the arrows B. A portion of the electrolyte solution introduced into the encapsulated anode flows out of the encapsulated anode through thebypass outlet 2016. By providing a dedicated bypass electrolyte solution supply into the encapsulated anode, the anode sludge or particulates generated from the dissolving anode is continually removed from the anode, thereby improving the purity of the electrolyte solution during the electroplating process. - FIG. 22 is a cross sectional view of yet another embodiment of an encapsulated anode. This embodiment of an encapsulated
anode 2000 includes ananode plate 2004, a plurality of electric feed-throughs 2006, atop encapsulation membrane 2008, abottom encapsulation membrane 2010, amembrane support ring 2012, and abypass outlet 2016. Theanode plate 2004 is secured and supported on the plurality of electric feed-throughs 2006. The top and abottom encapsulation membrane membrane support ring 2012. Thebypass outlet 2016 is connected to themembrane support ring 2012 and extends through thebowl 430. This embodiment of an encapsulated anode preferably comprises materials as described above for the previous-described embodiments of an encapsulated anode. Thebottom encapsulation membrane 2010 includes one ormore openings 2024 disposed substantially above the mainelectrolyte solution inlet 510. Eachopening 2024 is adapted to receive flow of electrolyte solution from the mainelectrolyte solution inlet 510 and is preferably about the same size as the internal circumference of the mainelectrolyte solution inlet 510. The flow of the electrolyte solution from the mainelectrolyte solution inlet 510, indicated by the arrow A, and the flow of the electrolyte solution within the encapsulated anode, indicated by the arrow B. A portion of the electrolyte solution flows out of the encapsulated anode through thebypass outlet 2016, carrying a portion of the anode sludge and particulates generated from anode dissolution. - FIG. 23 is a cross sectional view of another embodiment of an encapsulated anode. This embodiment of an encapsulated
anode 2000 includes ananode plate 2002, a plurality of electric feed-throughs 2006, atop encapsulation membrane 2008, abottom encapsulation membrane 2010, amembrane support ring 2012, and abypass fluid inlet 2014. Theanode plate 2002 is secured and supported on a plurality of electric feed-throughs 2006. The top andbottom encapsulation membranes membrane support ring 2012. Abypass fluid inlet 2014 is disposed through the bottom of thebowl 430 and through thebottom encapsulation membrane 2010 to introduce electrolyte solution into the gap between the encapsulation membranes and the anode plate. This embodiment of an encapsulated anode comprises materials as described above for the above-described embodiments of an encapsulated anode. In one embodiment, the flow of the electrolyte solution through thebypass fluid inlet 2014 and the mainelectrolyte solution inlet 510 are individually controlled bycontrol valves electrolyte solution inlet 510 is indicated by the arrows A while the flow of the electrolyte solution through the encapsulated anode is indicated by arrows B. For this embodiment, the anode sludge and particulates generated by the dissolving anode plate are filtered and trapped by the encapsulation membranes as the electrolyte solution passes through the membrane. - FIG. 16 is a schematic diagram of an electrolyte
solution replenishing system 220. The electrolytesolution replenishing system 220 provides the electrolyte solution to the electroplating process cells for the electroplating process. The electrolytesolution replenishing system 220 generally comprises a mainelectrolyte solution tank 602, adosing module 603, afiltration module 605, achemical analyzer module 616, and an electrolyte solutionwaste disposal system 622. The electrolyte solutionwaste disposal system 622 is connected to theanalyzing module 616 by an electrolytesolution waste drain 620. One or more controllers control the chemical composition of the electrolyte solution in themain tank 602 and the related operation of the electrolytesolution replenishing system 220. In one embodiment, the controllers are independently operable but integrated with thecontroller 222 of theECP system 200. - The main
electrolyte solution tank 602 provides a reservoir for electrolyte solution and includes an electrolytesolution supply line 612 that is connected to each of the electroplating process cells through one or more fluid pumps 608 andvalves 607. Aheat exchanger 624 or a heater/chiller disposed in thermal connection with themain tank 602 controls the temperature of the electrolyte solution stored in themain tank 602. Theheat exchanger 624 is connected to and operated by thecontroller 610. - The
dosing module 603 is connected to themain tank 602 by a supply line and includes a plurality ofsource tanks 606, or feed bottles, a plurality of valves 609, and acontroller 611. Thesource tanks 606 contain the chemicals needed for composing the electrolyte solution and typically include a deionized water source tank and copper sulfate (CuS0 4) source tank for composing the electrolyte solution.Other source tanks 606 may contain hydrogen sulfate (H2SO4), hydrogen chloride (HCl) and various additives such as glycol. Each source tank may be color coded and fitted with a unique mating outlet connector adapted to connect to a matching inlet connector in the dosing module. By color coding the source tanks and fitting the source tanks with unique connectors, errors caused by human operators when exchanging or replacing the source tanks are significantly reduced. - The deionized water source tank preferably also provides deionized water to the system for cleaning the system during maintenance. The valves609 associated with each
source tank 606 regulate the flow of chemicals to themain tank 602 and may be any of numerous commercially available valves such as butterfly valves, throttle valves and the like. Activation of the valves 609 is accomplished by thecontroller 611 which may be connected to thecontroller 222 to receive signals therefrom. - The electrolyte
solution filtration module 605 includes a plurality offilter tanks 604. An electrolytesolution return line 614 is connected between each of the process cells and one ormore filter tanks 604. Thefilter tanks 604 remove the undesired contents in the used electrolyte solution before returning the electrolyte solution to themain tank 602 for re-use. Themain tank 602 is also connected to thefilter tanks 604 to facilitate re-circulation and filtration of the electrolyte solution in themain tank 602. By re-circulating the electrolyte solution from themain tank 602 through thefilter tanks 604, the undesired contents in the electrolyte solution are continuously removed by thefilter tanks 604 to maintain a consistent level of purity. Additionally, re-circulating the electrolyte solution between themain tank 602 and thefiltration module 605 allows the various chemicals in the electrolyte solution to be thoroughly mixed. - The electrolyte
solution replenishing system 220 also includes achemical analyzer module 616 that provides real-time chemical analysis of the chemical composition of the electrolyte solution. Theanalyzer module 616 is fluidly coupled to themain tank 602 by asample line 613 and to thewaste disposal system 622 by anoutlet line 621. Theanalyzer module 616 generally comprises at least one analyzer and a controller to operate the analyzer. The number of analyzers required for a particular processing tool depends on the composition of the electrolyte solution. For example, while a first analyzer may be used to monitor the concentrations of organic substances, a second analyzer is needed for inorganic chemicals. In the specific embodiment shown in FIG. 16 thechemical analyzer module 616 comprises anauto titration analyzer 615 and a cyclic voltametric stripper (CVS) 617. Both analyzers are commercially available from various suppliers. An auto titration analyzer which may be used to advantage is available from Parker Systems and a cyclic voltametric stripper is available from ECI. Theauto titration analyzer 615 determines the concentrations of inorganic substances such as copper chloride and acid. The CVS 617 determines the concentrations of organic substances such as the various additives which may be used in the electrolyte solution and by-products resulting from the processing which are returned to themain tank 602 from the process cells. - The analyzer module shown FIG. 16 is merely illustrative. In another embodiment each analyzer may be coupled to the main electrolyte solution tank by a separate supply line and be operated by separate controllers. Persons skilled in the art will recognize other embodiments.
- In operation, a sample of electrolyte solution is flowed to the
analyzer module 616 via thesample line 613. Although the sample may be taken periodically, preferably a continuous flow of electrolyte solution is maintained to theanalyzer module 616. A portion of the sample is delivered to theauto titration analyzer 615 and a portion is delivered to the CVS 617 for the appropriate analysis. Thecontroller 619 initiates command signals to operate theanalyzers 615, 617 in order to generate data. The information from thechemical analyzers 615, 617 is then communicated to thecontroller 222. Thecontroller 222 processes the information and transmits signals that include user-defined chemical dosage parameters to thedosing controller 611. The received information is used to provide real-time adjustments to the source chemical replenishment rates by operating one or more of the valves 609. The received information thereby maintains a desired, and preferably constant, chemical composition of the electrolyte solution throughout the electroplating process. The waste electrolyte solution from the analyzer module is then flowed to thewaste disposal system 622 via theoutlet line 621. - Although one embodiment utilizes real-time monitoring and adjustments of the electrolyte solution, various alternatives may be employed. For example, the
dosing module 603 may be controlled manually by an operator observing the output values provided by thechemical analyzer module 616. In one embodiment, the system software allows for both an automatic real-time adjustment mode as well as an operator, manual, mode. Further, although multiple controllers are shown in FIG. 16, a single controller may be used to operate various components of the system such as thechemical analyzer module 616, thedosing module 603, and,theheat exchanger 624. Other embodiments will be apparent to those skilled in the art. - The electrolyte
solution replenishing system 220 also includes an electrolytesolution waste drain 620 connected to an electrolyte solutionwaste disposal system 622 for safe disposal of used electrolyte solutions, chemicals and other fluids used in the ECP system. In one embodiment, the electroplating cells include a direct line connection to the electrolytesolution waste drain 620, or the electrolyte solutionwaste disposal system 622. The electrolytesolution waste drain 620 drains the electroplating cells without returning the electrolyte solution through the electrolytesolution replenishing system 220. The electrolytesolution replenishing system 220 preferably also includes a bleed off connection to bleed off excess electrolyte solution to the electrolytesolution waste drain 620. - In one embodiment, the electrolyte
solution replenishing system 220 also includes one ormore degasser modules 630 adapted to remove undesirable gases from the electrolyte solution. The degasser module generally comprises a membrane that separates gases from the fluid passing through the degasser module and a vacuum system for removing the released gases. Thedegasser modules 630 are preferably placed in line on the electrolytesolution supply line 612 adjacent to theprocess cells 240. Thedegasser modules 630 are preferably positioned as close as possible to theprocess cells 240 so most of the gases from the electrolyte solution replenishing system are removed by the degasser modules before the electrolyte solution enters the process cells. In one embodiment, eachdegasser module 630 includes two outlets to supply degassed electrolyte solution to the twoprocess cells 240 of eachprocessing station 218. Alternatively, adegasser module 630 is provided for each process cell. The degasser modules can be placed at many other alternative positions. For example, the degasser module can be placed at other positions in the electrolyte solution replenishing system, such as along with the filter section or in a closed-loop system with the main tank or with the process cell. As another example, one degasser module is placed in line with the electrolytesolution supply line 612 to provide degassed electrolyte solution to all of theprocess cells 240 of the electrochemical plating system. Additionally, a separate degasser module is positioned in-line or in a closed-loop with the deionized water supply line and is dedicated for removing oxygen from the deionized water source. Because deionized water is used to rinse the processed substrates, free oxygen gases are preferable removed from the deionized water before reaching the SRD modules so that the electroplated copper is less likely to become oxidized by the rinsing process. Degasser modules are well known in the art and commercial embodiments are generally available and adaptable for use in a variety of applications. A commercially available degasser module is available from Millipore Corporation, located in Bedford, Mass. - One embodiment of the
degasser module 630, as shown in FIG. 26a, includes ahydrophobic membrane 632 having a fluid, i.e., electrolyte solution,passage 634 on one side of themembrane 632. Avacuum system 636 disposed on the opposite side of the membrane. Theenclosure 638 of the degasser module includes aninlet 640 and one ormore outlets 642. As the electrolyte solution passes through thedegasser module 630, the gases and other micro-bubbles in the electrolyte solution are separated from the electrolyte solution through the hydrophobic membrane and removed by the vacuum system. Another embodiment of thedegasser module 630′, as shown in FIG. 26b, includes a tube ofhydrophobic membrane 632′ and avacuum system 636 disposed around the tube ofhydrophobic membrane 632′. The electrolyte solution is introduced inside the tube of hydrophobic membrane, and as the electrolyte solution passes through thefluid passage 634 in the tube. The hydrophobic membrane separates gases and other micro-bubbles in the electrolyte solution, and a tube that is connected to thevacuum system 636 removes the separated gasses. More complex designs of degasser modules are contemplated, including designs having serpentine paths of the electrolyte solution across the membrane and other multi-sectioned designs of degasser modules. - Although not shown in FIG. 16, the electrolyte
solution replenishing system 220 may include a number of other components. For example, the electrolytesolution replenishing system 220 may also include one or more additional tanks for storage of chemicals for a substrate cleaning system, such as the SRD station. Double-contained piping for hazardous material connections may also be employed to provide safe transport of the chemicals throughout the system. Optionally, the electrolytesolution replenishing system 220 includes connections to additional or external electrolyte solution processing system to provide additional electrolyte solution supplies to the ECP system. - FIG. 17 is a cross sectional view of one embodiment of rapid thermal anneal (RTA) chamber. The
RTA chamber 211 is preferably connected to theloading station 210, and substrates are transferred into and out of theRTA chamber 211 by the loadingstation transfer robot 228. The ECP system, as shown in FIGS. 2 and 3, comprises twoRTA chambers 211 disposed on opposing sides of theloading station 210, corresponding to the symmetric design of theloading station 210. RTA chambers are generally well known in the art, and RTA chambers are typically utilized in substrate processing systems to enhance the properties of the deposited materials. A variety of RTA chamber designs, including hot plate designs and heat lamp designs, may be used to enhance the electroplating results. One RTA chamber is the WxZ chamber available from Applied materials, Inc., located in Santa Clara, Calif. Although this disclosure is described using a hot plate RTA chamber, other types of RTA chambers may be used as well. - Referring back to FIG. 2, the
ECP system 200 includes acontroller 222 that controls the functions of each component of the platform. In one embodiment, thecontroller 222 is mounted above themainframe 214, and the controller comprises a programmable microprocessor. The programmable microprocessor is typically programmed using a software designed specifically for controlling all components of theECP system 200. Thecontroller 222 also provides electric power to the components of the system and includes acontrol panel 223 that allows an operator to monitor and operate theECP system 200. Thecontrol panel 223, as shown in FIG. 2, is a stand-alone module that is connected to thecontroller 222 through a cable and provides easy access to an operator. Generally, thecontroller 222 coordinates the operations of theloading station 210, theRTA chamber 211, theSRD station 212, themainframe 214 and theprocessing stations 218. Additionally, thecontroller 222 coordinates with the controller of the electrolytesolution replenishing system 220 to provide the electrolyte solution for the electroplating process. - The following is a description of one embodiment of a substrate electroplating process sequence through the
electroplating system platform 200 as shown in FIG. 2. A substrate cassette containing a plurality of substrates is loaded into the substratecassette receiving areas 224 in theloading station 210 of theelectroplating system platform 200. A loadingstation transfer robot 228 picks up a substrate from a substrate slot in the substrate cassette and places the substrate in thesubstrate orientor 230. Thesubstrate orientor 230 determines and orients the substrate to a desired orientation for processing through the system. The loadingstation transfer robot 228 then transfers the oriented substrate from thesubstrate orientor 230 and positions the substrate in one of the substrate slots in the substrate pass-throughcassette 238 in theSRD station 212. Themainframe transfer robot 242 picks up the substrate from the substrate pass-throughcassette 238 and positions the substrate for transfer by theflipper robot 248. Theflipper robot 248 rotates its robot blade below the substrate and picks up substrate from mainframe transfer robot blade. The vacuum suction gripper on the flipper robot blade secures the substrate on the flipper robot blade, and the flipper robot flips the substrate from a face up position to a face down position. Theflipper robot 248 rotates and positions the substrate face down in thesubstrate holder assembly 450. The substrate is positioned below thesubstrate holder plate 464 but above thecathode contact ring 466. Theflipper robot 248 then releases the substrate to position the substrate into thecathode contact ring 466. Thesubstrate holder plate 464 moves toward the substrate and the vacuum chuck secures the substrate on thesubstrate holder plate 464. The bladder assembly 470 on thesubstrate holder assembly 450 exerts pressure against the substrate backside to ensure electric contact between the substrate plating surface and thecathode contact ring 466. - To limit deposition of metal film on the electric contacts, a negative bias is applied by the power supply702 (shown in FIG. 11) under the control of the
controller 222. Thehead assembly 452 is lowered to a processing position above theprocess cell 420. The negative bias voltage can then be applied to the electric contacts. The duration at which the negative bias voltage is applied to the electric contacts is shorter than a duration that would dry the electrolyte solution to form chemical (.e.g., copper sulfate) crystals on the electric contacts. As such, the duration at which the negative bias voltage may be applied to the electric contacts before immersion of the electric contacts and the substrate into the electrolyte solution is dependent on such factors as the particular chemical make-up of the electrolyte solution, and the drying conditions that the electric contacts are exposed to prior to immersion. During the immersion of the electric contacts into the electrolyte solution, however, a slight negative (depating) or neutral bias voltage is applied between the anode and the seed layer to ensure that the metal ions do not deposit on the electric contacts, maintaining the electric contacts in a pristine condition. The level of the slight negative or neutral bias voltage is selected to be insufficient to cause considerable deplating of the seed layer, or deposited metal film, on the substrate. At this position the substrate is below the upper plane of theweir 478 and contacts the electrolyte solution contained in theprocess cell 420. The power supply is activated to supply electric power, i.e., voltage and current, to the cathode and the anode to enable the electroplating process. The electrolyte solution is typically continually pumped into the process cell during the electroplating process. The electric power supplied to the cathode and the anode and the flow of the electrolyte solution are controlled by thecontroller 222 to achieve the desired electroplating results. In one embodiment, the head assembly is rotated as the head assembly is lowered and also during the electroplating process. - After the electroplating process is completed, the
head assembly 410 raises the substrate holder assembly and removes the substrate from the electrolyte solution. During removal of the substrate from the electrolyte solution, a slight negative (deplating) or neutral voltage is applied between the anode and the electric contacts to limit metal film deposition on the electric contacts. The level of the slight negative or neutral voltage is insufficient to cause deplating of the seed layer on the substrate. The exact level of the slight negative or neutral voltage is dependent upon the chemical make-up of the electrolyte solution. In one embodiment, the head assembly is spun for a period of time at a sufficient angular velocity such as between about 50 to about 3000 RPM, to enhance removal of residual electrolyte solution from the substrate and the substrate holder assembly. The vacuum chuck and the bladder assembly of the substrate holder assembly then release the substrate from the substrate holder plate. The substrate holder assembly is raised to allow the flipper robot blade to pick up the processed substrate from the cathode contact ring. The flipper robot rotates the flipper robot blade above the backside of the processed substrate in the cathode contact ring and picks up the substrate using the vacuum suction gripper on the flipper robot blade. The flipper robot rotates the flipper robot blade with the substrate out of the substrate holder assembly, flips the substrate from a face-down position to a face-up position, and positions the substrate on the mainframe transfer robot blade. The mainframe transfer robot then transfers and positions the processed substrate above theSRD module 236. The SRD substrate support lifts the substrate, and the mainframe transfer robot blade retracts away from theSRD module 236. The substrate is cleaned in the SRD module using deionized water or a combination of deionized water and a cleaning fluid as described in detail above. The substrate is then positioned for transfer out of the SRD module. The loadingstation transfer robot 228 picks up the substrate from theSRD module 236 and transfers the processed substrate into theRTA chamber 211 for an anneal treatment process to enhance the properties of the deposited materials. The annealed substrate is then transferred out of theRTA chamber 211 by theloading station robot 228 and placed back into the substrate cassette for removal from the ECP system. The above-described sequence can be carried out for a plurality of substrates substantially simultaneously in theECP system 200. Also, the ECP system can be adapted to provide multi-stack substrate processing. - 2. Voltage Levels Between the Anode and the Seed Laver
- The above describes an ECP system that is used to electroplate substrates. One concern during electroplating is to make the depth of metal film deposited across the substrate seed layer uniform. Metal film deposition can occur on the seed layer during the time that the substrate is being immersed in, or is being removed from the electrolyte solution. Most of the metal film deposition occurs when the seed layer on the substrate is fully immersed in the electrolyte solution. To ensure the uniformity of metal film deposition rate across the substrate seed layer, it is important to ensure that the electric current density applied to the seed layer is uniform across the face of the substrate. One aspect of the. ECP system that increases the uniformity of electric current density applied to the substrate seed layer is ensuring that each one of the plurality of electric contacts remains consistently pristine. A method of modulating the power supply is described herein so that the, electric contacts are maintained in a pristine state substantially free of metal film deposition, oxidation, or the chemical crystals that can occur when the power supply is off. Additionally, the modulation of the power supply enhances uniform deposition of the metal film on the seed layer.
- The
controller 222 controls the level of voltage/current applied between the anode and the seed layer on the substrate that is produced by a power supply. For plating consideration, the voltage level of the seed layer is considered relative to the anode through the electrolyte solution. FIG. 27 shows one embodiment of plating process depicted by a graph 2700 with voltage plotted as the ordinate 2702 versus time plotted as theabscissa 2704 during the plating process. Any voltage level above the level of theabscissa 2704 indicates a positive voltage of the substrate seed layer relative to the anode, i.e., an anodic seed layer and a cathodic anode. Any voltage level below theabscissa 2704 indicates a negative voltage level of the seed layer relative to the anode, i.e., a cathodic substrate seed layer and an anodic anode. A reverse bias voltage exists where the voltage of the substrate seed layer is greater than the voltage level of the anode. Therefore, a reverse bias voltage represents a reverse polarity between the anode and the seed layer as compared to the polarity of a plating voltage. During etching portions of the plating process, greater reverse bias typically results in a greater etch rate of the substrate seed layer. -
Reference character 2720 represents one plating voltage cycle for a given substrate within an electrolyte cell during the plating process. Each platingvoltage cycle 2720 includes a reverse bias voltage, also known as a metal film etch portion 2708, indicated as 2708 a or 2708 b, and a plating voltage, i.e., metal film deposition,portion 2714. Theplating voltage portion 2714 represents the voltage level when a plating voltage is applied between the anode and the substrate seed layer. During theplating voltage portion 2714, the metal ions in the electrolyte solution are deposited on the substrate seed layer to form a metal film. The duration of the plating voltage portion is a function of the chemical make-up of the electrolyte solution, the metal being used in the ECP process, the desired thickness of the metal film deposited on the seed layer, and other such factors. The duration of the plating voltage portion may range from about 10 seconds to several minutes or more depending upon the chemical make-up of the electrolyte solution, i.e., the recipe used during the ECP process. The voltage level of theplating voltage portion 2714 may range from a fraction of a volt to 10 or more volts. - The reverse bias voltage2708 is applied as the substrate is being immersed into, or withdrawn from, the electrolyte solution. The reverse bias voltage also exists between plating cycles such as when there is a temporary production downtime. Such downtime exists when no more substrates are being processed in the ECP system for some prescribed duration, .e.g., five minutes or longer. During such ECP system downtime, it is common to immerse the substrate holder assembly, including.the electric contacts, in the electrolyte solution contained in the electrolyte cell. Such immersion of the electric contacts limit evaporation of the electrolyte solution on the electric contacts that would otherwise form as chemical, .e.g., copper sulfate, crystals.
Voltage level 2708 a represents that portion of the reverse bias voltage that is applied during a metal film etch platingvoltage cycle 2720 when substrates are being immersed into, or removed from, the electrolyte solution. Such reverse bias voltage, e.g., metal film etch, portions of the cycle are applied typically for a relatively brief duration of time, typically less than 30 seconds. During the time that the reverse bias voltage portion 2708 of each cycle is being applied: a) a first substrate is removed from the electroplating cell, b) a robot removes the first substrate from the substrate holder assembly, c) a robot inserts a second substrate into the substrate holder assembly, and d) thesubstrate holder system 14 immerses the second substrate into the electroplating process cell. It is common for each substrate to undergo multiple plating cycles intermixed with multiple etching or cleaning cycles ECP processing. The voltage level of thereverse bias voltage 2708 a may vary as a function of the dimensions of the electrolyte cell, the composition of the electrolyte solution, the metal film, and the seed layer, etc. The substrate seed layer is typically biased anodically relative to the anode by, e.g., about a fraction of a volt to about 4 volts during whenvoltage level 2708 a is applied. - The reverse
bias voltage portion 2708 b is applied between the anode and the seed layer for an extended duration when substrates are not being processed. Such lack of processing down time may extend from a fraction of a minute to a day or more when no substrates are being plated. In this disclosure, the term “down time” is applied to these extended periods no substrates are being processed by the ECP system. To provide a consistent electric current density across the face of the substrate during metal film deposition on the substrate, it is important to ensure that the electric contacts are pristine. In this disclosure, the term “pristine” means that the electric contacts are substantially free of electroplated metal deposits and/or dried chemical crystals during ECP processing. During extended down-time periods when no substrate is in the substrate holder, the substrate holder assembly is positioned so all of the electric contacts are immersed in the electrolyte solution. This immersion during down time limits an oxidation reaction that results when the electric contacts are exposed to the oxygen present in the atmosphere. The voltage level that has to be applied to the anode and the seed layer during thereverse bias portion 2708 b is a function of the dimensions of the electrolyte cell, the chemical composition of the electrolyte solution and/or the seed layer, etc. However, a typical voltage level of thereverse bias portion 2708 b for copper electroplating has the contact elements biased anodically relative to the anode by about a fraction of a volt to about 4 volts. - When the substrate is being prepared to be immersed into the electrolyte solution after the extended reverse
bias voltage portion 2708 b, the substrate seed layer continues to be reverse biased by having positive voltage 2708, relative to the anode as a time extension of the reversebias voltage portion 2708 b during the immersion. Thisreverse bias 2708 b during immersion serves a similar function as the reverse bias voltage of 2708 a. The substrate holder assembly then immerses the seed layer into the electrolyte solution until the seed layer is fully immersed in the electrolyte solution. A closed electric circuit is created between the anode and the seed layer as the substrate is being immersed. The electric current is a function of the voltage between the anode and the seed layer and the amount that the seed layer that has been immersed. The reverse-bias voltage 2708 b is maintained until the substrate has been fully immersed into the electrolyte solution at 2710, then the anode and the seed layer are switched to a normal bias voltage as shown by 2714. - The substrate generally is immersed in a horizontal orientation into the electrolyte solution with the seed layer facing down. In certain embodiments, the substrate may be tilted from horizontal within the substrate holder assembly during immersion. Such tilting provides for removal of air or air bubbles that may otherwise be trapped within the electrolyte solution underneath portions of the substrate holder assembly and/or substrate, during the immersion process. Closely following the full immersion of the substrate seed layer, the voltage between the anode and the seed layer is changed from a positive (reverse bias) voltage to a negative (normal bias) voltage. The negative normal bias voltage of the anode relative to the seed layer, via the electrolyte solution, is sufficient to cause metal ions in the electrolyte solution to deposit metal film on the seed layer. Such a negative normal bias voltage of the anode relative to the seed layer is known as “plating voltage”. The plating voltage typically follows a plating recipe that is a function of the chemicals in the electrolyte solution, the dimensions of the substrate and the anode, etc.
- The
reverse bias voltage 2708 a limits metal ions being deposited as metal film on the substrate seed layer. During the immersion of the substrate into the electrolyte solution, thereverse bias voltage 2708 a is applied to limit certain portions of the seed layer from being coated more heavily by metal film than other seed layer portions. Such irregular coating may result from, e.g., irregular electrolyte solution flow about the substrate seed layer during immersion of and/or removal of the substrate at an angle from horizontal. As such, thereverse bias voltage 2708 a limits uneven metal film deposition on the seed layer that may result during the immersion and/or removal of the substrate from the electrolyte solution. Alternatively, the voltage of the anode may be set equal to the voltage of the seed layer to limit both excessive deposition or etching of the metal film on the seed layer. If neither a plating voltage nor a deplating voltage is applied to the substrate seed layer, while little deposition to the seed layer occurs, little etching occurs. The duration from when the first portion of the seed layer is immersed to when the substrate is fully immersed is quite rapid, usually under three seconds, during which time a slight reverse bias is applied. - When the voltage of the seed layer is greater than the voltage of the anode, the ions in the electrolyte solution are not attracted to the seed layer in sufficient quantities to effect plating. However, certain embodiments of electrolyte solution has a low pH, i.e., acidic, as these embodiments contain a considerable amount of hydrochloric acid. Since such an electrolyte solution itself is acidic, it will slightly etch (deplate) the seed layer and/or the metal film metal if no voltage is applied between the anode and the substrate. Thus, it might also make sense to apply a very low plating voltage during substrate immersion.
- The metal film deposition process is a function of the bias voltage applied between the anode and the seed layer on the substrate. As positively charged copper ions are deposited to form the metal film on the negatively charged substrate seed layer by the plating voltage, the copper ions from the depletion regions are depleted. However, an atom-level electronic exchange, associated with the chemical reaction of the anode in the electrolyte solution current, drives copper atoms contained in the anode into the electrolyte solution from the anode. Thus, the anode in many embodiments includes a solid piece of copper. The
plating voltage portion 2714 can actually be a series of prescribed voltage levels with the voltage levels and the durations selected as a function of the composition of the electrolyte solution. The voltage levels and durations depend on such factors as the electrolyte solution being used, the distance between the anode and the seed layer, the dimension of the electrolyte cell and the substrate, and the desired metal film deposition thickness. Alternatively, theplating voltage portion 2714 can be arranged as a series of plating voltages alternating with a series of etching voltages. The etching voltages can be applied, e.g., to keep openings or “throats” of features formed in the substrate seed layer open so the features can be more completely filled during the plating voltages. - The chemical reaction embodiments that may occur in the embodiment of ECP system shown in FIGS.1 or 6 may be characterized by whether a positive bias is applied between the anode and the seed layer to effect plating metal film on the substrate, or whether a negative bias is applied between the anode and the seed layer to effect deplating metal film on the substrate. If a sufficient positive bias is applied so the voltage of the seed layer is below the voltage of the anode to effect plating on the substrate the following exemplary chemical reactions occur:
- The anode chemical reaction is:
- 2H2O→O2+4H++4e−
- The cathode (seed layer) chemical reaction is:
- Cu+++2e−→Cu
- If a sufficient negative bias is applied so the voltage of the seed layer exceeds the voltage of the anode by a sufficient level to effect deplating copper from the seed layer, the following exemplary chemical reactions occur:
- The anode chemical reaction is:
- Cu→Cu+++2e−
- The cathode (seed layer) chemical reaction is:
- Cu+++2e−→Cu
- The voltage of the electrolyte solution adjacent the substrate seed layer is relatively small, e.g., about 1 volt. The copper ions therefore arrive at the seed layer surface primarily by diffusion within the electrolyte solution. The voltage level of the seed layer controls the rate at which the copper ions deposit on the substrate seed layer to form a metal film. Higher voltages established between the anode and the substrate seed layer force more ions into the electrolyte solution as a result of increasing the chemical reaction between the anode and the seed layer. The higher voltage levels result in a higher deposition rate of metal ions onto the substrate seed layer since a higher concentration of copper is contained in the electrolyte solution due to the increased chemical reaction between the anode and the electrolyte solution.
- Increasing the voltage level between the anode and the seed layer affects the deposition rate of the seed layer only up to the level of the diffusion limit, at which level all of the diffused ions are converted into copper ions. Above the diffusion limit, a further increase in the voltage between the anode and the seed layer breaks the bonds of the water in the electrolyte solution and does not improve the deposition rate of the metal film on the seed layer.
- FIGS. 28 and 29, show one embodiment of
method 2800 performed by thecontroller 222 that controls the electric current/voltage applied from the anode to the seed layer, in which a substrate is immersed into the electrolyte solution contained in the electrolyte cell during eachvoltage cycle 2720.Method 2800 includes a relatively brief reversebias voltage portion 2708 a being applied between the anode and the substrate seed layer. Themethod 2800 is discussed in relation with the voltage cycle shown in FIG. 27.Method 2800 starts with block 2802 in which the substrate holder assembly, that holds the substrate in a position such that the substrate is removed from the electrolyte solution contained within the electrolyte cell, starts spinning the substrate in at an angular velocity of less than about 100 RPM (commonly under 30 RPM) preparation of the substrate being immersed in the electrolyte solution. The spinning is performed only on those substrate holder systems that are configured to spin the substrate such as, e.g., the embodiment shown in FIG. 25. Certain substrate holder systems, such as shown in the embodiment of FIG. 1, are not configured to rotate the substrate. Such spinning occurs, in certain embodiments, within the neutral voltage period 2706. The period 2706 may be applied for a prescribed period after eachplating voltage portion 2714 that is sufficient to remove the liquid from the surface of the substrate by centrifugal action. -
Method 2800 continues to block 2804 in which the controller applies the reverse bias voltage portion, 2708 a as shown in FIG. 27, between the anode and the seed layer. The voltage level of the seed layer equals, or is more positive than, the voltage level of the anode during the reversebias voltage portion 2708 a. As such, the seed layer is actually slightly anodic relative to the anode during the reverse bias voltage. The positive voltage level of the anode relative to the seed layer is of an insufficient voltage, and applied for an insufficient duration, to cause considerable etching of the seed layer and/or the metal film deposited on the seed layer. When the seed layer on the substrate does not contact the electrolyte solution in the electrolyte cell, an open circuit exists since no medium is carrying electric current between the anode and the seed layer. Any voltage differences between the anode and the seed layer does not result in an associated current flow as long as the substrate seed layer is removed from the electrolyte solution since no current path exists between the anode and the seed layer. - The
method 2800 continues to block 2806 in which the substrate holder system immerses the substrate seed layer into the electrolyte solution. As soon as any portion of the seed layer is immersed in the electrolyte solution, a closed circuit is formed between the anode and those portions of the seed layer that are immersed. The immersion process is performed quickly in one embodiment to limit any undesired, or uneven etching that may occur on the substrate as the reversebias voltage portion 2708 a is applied between the anode and the seed layer. Such limiting of the deposition during immersion is desired since portions of the substrate may not be immersed early during the immersion process. For example, certain embodiments of substrate holder systems immerse the substrate in the electrolyte solution in a tilted position wherein the substrate is angled from horizontal. In these embodiments of substrate holder systems, peripheral parts of the tilted seed layer on the substrate are immersed before other seed layer parts. The reverse bias applied between the anode and the seed layer limits the plating that occurs on the seed layer during the immersion process. Themethod 2800 continues to block 2808 after full immersion, in which theplating voltage portion 2714 is applied between the anode and the seed layer. Since the seed layer is immersed in the electrolyte solution, a closed circuit is formed between the anode and the seed layer. The substrate seed layer is thereby cathodic relative to the anode. The deposition rate of metal film on the seed layer on the substrate is a function of the current density applied to the seed layer. The current density on the seed layer is a function of the current flow between the anode to the seed layer. The current from the anode to the seed layer, in turn, is a function of the voltage between the anode and the seed layer. Therefore, thecontroller 222 can control the deposition rate of a metal film on the seed layer by controlling the voltage level applied by a power supply between the anode and the seed layer. Duringblock 2808, the seed layer on the substrate is processed, i.e., electroplated, at which time a metal film is deposited on the substrate. - The
method 2800 continues to block 2814 in which the substrate held in the electrolyte cell by thesubstrate holder system 14 completes the metal film deposition using plating voltage between the anode and the seed layer, such as theplating voltage portion 2714 shown in FIG. 27. Themethod 2800 continues to block 2816 in which the controller appliesreverse bias voltage 2708A between the anode and the seed layer. The duration of the reverse bias voltage in block 2816 is envisioned to be sufficient for a first substrate to be removed from the electrolyte solution, for a second substrate to be positioned within the substrate holder assembly, and for the second substrate to be immersed into the electrolyte solution. Themethod 2800 then continues to block 2818 in which the substrate is removed from the process cell. During the removal of the substrate from the process cell, the reverse bias voltage will be sufficient to limit excessive deposits forming on either the substrate seed layer, or the electric contact within the substrate holder assembly. The duration in which the substrate and the electric contacts are completely removed from the electrolyte solution within the process cell is relatively brief to limit the electrolyte solution drying on the face of the seed layer on the substrate or on the electric contacts. Such limiting of the electrolyte solution drying on the electric contacts also limits a crystalline coating containing copper sulfate from forming on the electric contacts that would alter the electric properties of the electric contacts. - The
method 2800 then continues to decision block 2820 in which the controller determines if there is another substrate that is ready to be processed. If the answer to decision block 2820 is no, then themethod 2800 continues to block 2822. In block 2822, thecontroller 222 performs a loop withdecision block 2910, in which controller waits and applies thereverse bias voltage 2708 b until the next substrate is ready to be inserted within the substrate holder assembly into the electrolyte solution. As thereverse bias voltage 2708 b is applied, the substrate holder system holds the electric contacts in an immersed position in the electrolyte solution. Immersing the electric contacts into the electrolyte solution during down time limits the exposure of the electric contacts to air, and thereby limits the oxidation of the electric contacts. Additionally, immersing the electric contacts into the electrolyte solution during down time limits the evaporation of the electrolyte solution onto the surface of the electric contacts. The evaporation of the water in the electrolyte solution on the electric contacts would result in the coating of the electric contacts with the copper sulfate in the electrolyte solution. During the immersion of the electric contacts into the electrolyte solution, the application of thereverse bias voltage 2708 b is also sufficient to limit the deposition of copper from the electrolyte solution onto the electric contacts. - If the answer to decision block2820 is yes, then the
method 2800 loops back to block 2801.Method 2800 loops continuously to perform the waveform described relative to FIG. 27 on successive substrates. The user can input information to thecontroller 222 if it is desired to discontinue themethod 2800 at any point. - While the foregoing is directed to the preferred embodiment of the present invention, other and further embodiments of the invention may be devised without departing from the basic scope thereof.
Claims (25)
1. A method for immersing a substrate into a processing solution, comprising:
connecting a power supply between a conductive layer on the substrate and an electrode positioned in the processing solution;
immersing the substrate into the processing solution; and
applying a forward electrical bias to the conductive layer during the immersion.
2. The method of claim 1 , wherein the forward bias is a plating bias configured to deposit metal ions in the processing solution onto the conductive layer.
3. The method of claim 2 , wherein the forward bias is a low plating bias.
4. The method of claim 3 , wherein the processing solution is an electrochemical plating solution.
5. The method of claim 4 , wherein the conductive layer is a seed layer.
6. The method of claim 5 , wherein immersing further comprises rotating the substrate.
7. The method of claim 5 , wherein immersing further comprises tilting the substrate.
8. The method of claim 1 , wherein applying the electrical bias comprises applying a plating bias to the conductive layer sufficient to overcome etching of the conductive layer by the processing solution.
9. The method of claim 1 , wherein the electrical bias is configured such that the conductive layer is at a lower electrical potential than the anode.
10. The method of claim 1 , comprising continuing the application of the electrical bias until a forward plating bias is applied to the conductive layer.
11. A method for immersing a substrate into an electrochemical plating solution, comprising:
electrically connecting a seed layer on the substrate with a first terminal of a power supply;
electrically connecting an anode positioned in the electrochemical plating solution to a second terminal of a power supply;
immersing the substrate into the electrochemical plating solution; and
applying an electrical bias between the first terminal and second terminal during the immersing.
12. The method of claim 11 , wherein the electrical bias is a low plating voltage.
13. The method of claim 11 , wherein the electrical bias is configured such that the first terminal has a lower electrical potential than the second terminal.
14. The method of claim 11 , further comprising rotating the substrate during the immersion.
15. The method of claim 11 , further comprising tilting the substrate during the immersion.
16. The method of claim 11 , further comprising rotating and tilting the substrate during the immersion.
17. The method of claim 11 , wherein the electrical bias is a forward bias configured to prevent etching of the seed layer by the electrochemical plating solution.
18. The method of claim 1 1, wherein the electrolyte solution has a pH of less than about 5.
19. The method of claim 11 , comprising continuing the application of the electrical bias after the immersion until a plating bias is applied.
20. A method for immersing a substrate into an electrochemical plating cell, comprising:
securing the substrate to an electrical contact element;
rotating the substrate;
immersing the substrate into a plating solution contained in the electrochemical plating cell;
applying an immersion bias to the substrate during the immersing;
applying a plating bias after the substrate is immersed in the plating solution.
21. The method of claim 20 , comprising tilting the substrate during the immersion process.
22. The method of claim 21 , comprising positioning the substrate horizontally before increasing the immersion bias to the plating bias.
23. The method of claim 20 , wherein the immersion bias is a forward bias.
24. The method of claim 23 , wherein the forward bias is a low plating bias.
25. The method of claim 20 , comprising continuing the immersion bias until the plating bias is applied.