CA2181163C - Cold caustic extraction of pulps for absorbent products - Google Patents

Cold caustic extraction of pulps for absorbent products Download PDF

Info

Publication number
CA2181163C
CA2181163C CA002181163A CA2181163A CA2181163C CA 2181163 C CA2181163 C CA 2181163C CA 002181163 A CA002181163 A CA 002181163A CA 2181163 A CA2181163 A CA 2181163A CA 2181163 C CA2181163 C CA 2181163C
Authority
CA
Canada
Prior art keywords
pulp
cold
extraction
pulps
alkali
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired - Fee Related
Application number
CA002181163A
Other languages
French (fr)
Other versions
CA2181163A1 (en
Inventor
Phyllis Leithem
Charles A. Kremers
Paul W. Harrell
Stephen Lewis
Karl D. Sears
Quan He
Peter R. Abitz
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Rayonier Inc
Original Assignee
Rayonier Inc
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Rayonier Inc filed Critical Rayonier Inc
Publication of CA2181163A1 publication Critical patent/CA2181163A1/en
Application granted granted Critical
Publication of CA2181163C publication Critical patent/CA2181163C/en
Anticipated expiration legal-status Critical
Expired - Fee Related legal-status Critical Current

Abstract

An improved absorbency material for absorbency applications comprised of a cellulosic fibrous material wherein said cellulosic fibro us material such as pulp is a cold alkali solution treated material at a treatment temperature of less than about 50 .degree.C; a proce ss for improving absorbency and other characteristics of said pulp.

Description

= WO 95120066 21v 1163 PCT/US95/00862 3 SPECIFICATION _ 4 This invention relates to pulps for absorbent products, more particularly this invention relates to novel use of modified pulps for absorbent 6 products of household and hygienic uses such as diapers, incontinence and 7 catamenial devices and the like and a method for preparing puips of outstanding 8 absorbency characteristics.
9 More particularly, this invention relates to the novel use of known technology - cold alkali extraction - to produce cellulosic pulps having altered and 11 novel fiber properties desirable for end-use applications for absorbent and fluff pulp 12 products.

13 Further, this invention relates to the production of the altered and 14 novel pulps without addition of chemical additives such as sheet debonders.
Still further this invention relates to 'the production of pulps having novel, desirable 16 properties achieved without chemical modification steps such as cross-linking with 17 chemical cross-linking agents.

18 Moreover, this invention relates to a novel use of a pulp product 19 characterized and defined by its properties for suitable end uses of these pulps.
Accordingly, novel pulp products can be obtained at reduced cost for the 21 respective, economic effectiveriess of these pulps when compared to pulps 22 prepared by the prior art and suitable for the same purpose.

24 With the increasing prominence of disposable items, such as diapers, paper towels and the like, and in view of the widely prevalent use of 26 absorbent tissues of various kinds, it has become important to obtain putps of high 27 absorbency, especially pulps tlhat display high absorbency upon multiple re-28 wetting.

CA 02181163 2003-07-09 =
_') _ 1 Typically pulps that are used for hygienic absorption purposes such 2 as baby diapers and the like are constructed with an outside "acquisition"
layer, 3 which is a layer of pulp of good bulking properties and good absorbency due to 4 relative fiber stiffness. A bulky material will contain a high percentage of void spaces or pores. For an absorbent product, these pores are used to acquire, 6 transport and store fluid. Longer, stiffer fibers make bulkier air laid webs with more 7 pore volume. Fluids are more easily acquired and transported if pore volume or 8 bulk is high. The "acquisition" layer is positioned between the baby's skin and the 9 absorbent core of the diaper. An "acquisition" layer of proper characteristics and properties allows the liquid to pass quickly into the absorbent core upon repeated 11 wettings and at the same time this layer transmits the liquid into the principal 12 absorbent core that holds the liquid. In a similar manner, an incontinent or 13 catamenial device may be constructed. Further, wound dressing material may be 14 construed in a like manner. These devices are absorbency products which require pulps having intensive absorbency properties.

16 Still further, absorbent multi-ply papers such as household towels 17 may be constructed of multiple layers or plies including a core layer and thus 18 these plies may be tailored according to the use to which these goods are being 19 subjected or for the purpose these are employed.

Products such as diapers when used with an outside "acquisition"
21 layer and an interior principal absorbent core, are presently desirably constructed 22 with the "acquisition" layer made from cross-linked pulps such as are illustrated by 23 the following European Patent applications 0 427,316 A2 and 0 427,317 A2 all by 24 Herron et al. and U.S. Patent no. 5,137,537 by Herron et al. assigned to Proctor &
Gamble Co. Further, Canadian Patent application 2,035,402, by Kokko 1 assigned to James River Corp. likewise discloses such pulps.

3 Cross-linked pulps are typically prepared using formaldehyde=-based 4 compounds. More recently, polycarboxylic acids, particularly citric acid, have been shown to be effective cross-linking agents. Cross-linked fibers display excellent 6 wet stiffness. The cross-links physically restrict the uptake of water into the fiber 7 wall. By doing so, the fiber retains, better than conventional fiber, the 8 characteristic stiffness of dry fibers. A web of cross-linked fibers, therefore, retains 9 its bulk and pore volume when wet, which enhances fluid acquisition, especially with repeated wettings or insults. However, chemically cross-linked fibers are 11 considerably more expensive than fibers which may be employed without any 12 cross-linking. Moreover, pulps employed in prior art processes for cross-linking 13 purposes are generally not available in sheeted form (rolls or bales of sheets).
14 Although pulps have been bleached under various alkaline conditions, bleaching schedules and bleaching treatment are by now those 16 typically employed by prior art. Accordingly, a wide variety of such schedules are 17 practiced -- for the most part employing at least one or more alkaline steps at fairly 18 high temperatures. In such sequences it has also been known to employ caustic 19 solutions at lower temperature and then the same solution is used to bring up the temperature to or greater than a boiling point of the solution as shown in Canadian 21 Patent 578,573 entitled "Purification of Wood Pulp" granted June 30, 1959.
In this 22 patent the pulps so produced are used for dissolving pulps, i.e., making cellulose 23 acetate and other chemical derivatives of cellulose. No description has been 24 found concerning the improvements in absorbency, rewetting properties, stiffness of fibers, etc. as described herein for the pulps as used for the devices or products 1. as illustrated herein. Moreover, the distinction between dissolving pulps and fluff 2 pulp should also be noted.

4 With reference to the Drawing herein:

Figure 1 is a plan view of a typical baby diaper;

6 Figure 2 is a cross-sectional view of the diaper shown in Figure 1, 7 along lines 2-2 thereof; and 8 Figure 3 is a schematic self-explanatory presentation of the overall 9 process/product improvements.

BRIEF DESCRIPTION OF THE INVENTION

11 According to the present invention there is provided an absorbent 12 article comprising a fluffed alkali treated absorbent pulp which is without chemical 13 crosslinking covered with a fluid permeable topsheet characterized in that the 14 alkali treated absorbent pulp is produced by suspending a cellulosic pulp in an alkali solution of a concentration from 3% to 25% by weight for a treatment time 16 from five minutes to one hour at a temperature below 60 C, recovering the alkali 17 treated pulp from the suspension, drying the alkali treated pulp and fluffing the 18 dried alkali treated pulp.

- 4a -It has been found that cold alkali extraction (CAE) of pulps such as preferably obtained from coniferous and deciduous trees results in fibers that have advantageously and unexpectedly improved absorption properties.

Pulps from other source materials may also be suitable (e.g., bagasse, straw, etc.).
By the term "cold" it is meant a caustic treatment not to exceed 60 C but desirably at a temperature less than 50 C but preferably at a temperature between 15 C
to 40 C. Cold alkali extraction is synononous with cold caustic extraction CCE
when caustic is used as the alkali source. By the term "caustic" it is meant sodium hydroxide solutions newly made up or as a solution by-product in a pulp or paper mill operation e.g., hemi caustic white liquor, oxidized white liquor and the like.
Further, ammonium hydroxide, and potassium hydroxide and the like may be employed. However, from a cost standpoint, the preferable caustic material is sodium hydroxide. Cold alkali extraction may be performed with additional chemicals added such as hydrogen peroxide, sodium hypochlorite, sodium borohydride, various surfactants, etc.

eol*' = WO 95120066 218116 7 PCT/US95/00862 1 The cold caustic extraction is typically at a caustic strength in a 2 range from about 3% to 25%, preferably from about 6% to 18%, at a pulp 3 consistency from about 2% to 25% but desirably from 2% to 10% but preferabiy 4 from 3% to 8%. Pulps for high rate, fast absorbing applications are preferably treated with cold caustic concentrations from 13% to 18%. A wide variety of pulps 6 are suitable such as obtained by mechanical or chemi-mechanical, sulfite, kraft, 7 pulping reject materials, organic solvent pulps, etc. Both softwood and hardwood 8 species are useful. Softwood pulps are preferred. Among pulps those that have 9 not been severely bleached are useful, for example pulps with high K Numbers (i.e., "potassium permanganate" number; a high K or Kappa Number signifies a 11 relatively high residual lignin content for the pulp). The more heavily bleached pulp 12 will be improved less and also irequires a weaker alkali treatment. If the pulps are 13 treated in the manner as it will be further disclosed in the specification herein, then 14 the resulting fibers are such that these have good bulking, (i.e., "stiffness"

properties) and thus have much improved absorption and rewetting properties 16 making these pulps attractive for a number of uses. These pulps are not only 17 characterized for their improveci properties, such as by their ability to absorb and 18 reabsorb water more quickly (ttian the standard untreated pulps) when subjected 19 to multiple rewet tests, but also these pulps are useful for absorbent devices in the principal core for such device. In fact, the resulting improvements in the 21 absorption properties are so significant that the products on an economical basis 22 may readily compete with the more expensive prior art cross-linked products 23 described in the above-identified patents.

24 As mentioned above, the newly discovered pulp preparation has wide applicability to all types oV pulp/fiber source materials and displays improved 26 properties for each of the pulps/fibers (Figure 3). Upon a cold caustic treatment of WO 95120066 '218116Z' PCT/US95/00862 -6..-d 1 the pulp/fibers, these show improved properties. For pulps prepared under 2 different pulping conditions or processes such as sulfite, pre-hydrolyzed kraft 3 process, conventional kraft process, organic solvent processes, or BCTMP

4 (bleached chemi-thermal mechanical pulp), etc., the properties are invariably improved. The improved properties have been observed for all pulp and fiber 6 types investigated. Differences, however, exist between pulps obtained from 7 various wood species starting materials. Surprisingly, the improved properties are 8 obtained regardless of the wood species which have been employed, for example, 9 western hemlock, Douglas fir, Sitka spruce, Southern pine, Caribbean pine and the like. Other commercial softwood species (e.g., firs and spruces) and hardwood 11 species (e.g., gums, oaks, eucalyptus, poplar, beech, aspen, etc.) yield 12 advantageous properties as well.

13 In an advantageous embodiment, it seems that the best 14 characteristics for the obtained pulp have been observed for pulps that are unbleached or only slightly bleached. Nevertheless, good results have also been 16 observed with bleached or more highly bleached pulps. As a corollary, the more 17 highly bleached is the pulp, the lower is the caustic strength that is required to 18 obtain the desirable effects. However, the desirable absorbency effects are 19 somewhat less when compared on a direct basis with cold caustic extracted pulps derived from high K Number unbleached pulps (i.e. the products derived from high 21 K Number pulps are noticeably better).

22 With reference to an embodiment, and the drawing herein, a typical 23 construction of a diaper is shown in Figures 1 and 2 therein. In Figure 1 the plan 24 view of the diaper 3 in its open position shows the tabs 4 which are a part of a hook or loop component shown as 5 as its complementary element. Other diaper 26 designs include tape-fasteners.

= WO 95/20066 218r 163 PCT/US95/00862 1 In Figure 2 which shows in cross section along lines 2-2 of Figure 1 2 the construction features of diaper 3 and with reference thereto from top to bottom 3 each element in the cross section 2-2 is described as follows:

4 Item 11 is a thermally-bonded polypropylene coversheet. It is typically carded or spun. Item 12 is an airlaid cellulose acquisition layer.
Elements 6 13 are tissue webs of a typical basis weight of about 16 g/m2; the absorbent core 7 is identified as 14 and is of a fluff and SAP (super absorbent polymer and pulp 8 mixture of a basis weight of, 500 - 700 g/m). The water barrier, which is a 9 polyethylene sheet has been sihown as 16.

While the above illustration has been for a diaper, other devices 11 have been constructed in a similar manner. Further, for similar absorbent paper 12 products, the pulps as modified herein show substantial improvement in product 13 performance on an economical basis. Thus, products such as catamenial and 14 incontinence devices are improved. Other candidate applications for which the presently disclosed pulps are suitable are paper towels, sanitary tissue papers, 16 industrial wipes, etc. For the above applications, the modified pulps may be 100%
17 of the improved pulps as constituent pulps in the product or may be used in the 18 product in lesser quantities, i.e., used in various admixtures with other pulp, from 19 about 100% to about 25%.

Test Procedures 21 Whenever these tests have been described, the industry employed 22 standard test procedure for the test has been used. If any changes in the 23 procedure have been made, the changes have been described specifically.

24 For purposes of evaluating the pulps obtained and described by the present disclosure as well as the invention herein, several tests were used to 26 characterize the desirable fibrous end-use performance improvements resulting -g-i from the use of cold alkali extraction and to describe some of the analytical 2 properties of the pulp products. Also, some of the terminology used in discussing 3 the products in the examples has been defined.

4 A summary of these tests and definitions follows.
Pulp Analvtical Properties 6 The K Number or Kappa test is carried out according to TAPPI

7 Standard Method No. T-214-SU71. This test is a measure of residual lignin content 8 in the pulp. The test indicates the relative degree of residual lignin content in a 9 pulp as a consequence of pulping and the extent or severity of pulping.

Pulp brightness is a measure of pulp whiteness with 100% being the 11 maximum. Pulp brightness data here are given as ISO brightness values in %.

12 The ISO brightness test is described in Tappi Method Number T272 (Handsheets) 13 and T525 (Instrumentation) and uses as a measuring device a Datacolor 2000T""
14 brightness meter.

Pulp Sheet Properties 16 Debonded pulps are fibrous end-use pulps (for example, fluff pulps) 17 that have some chemical agent (debonder) added to inhibit interflber bonding 18 (addition of debonder results in a soft pulp sheet). The chemical agents, 19 debonders, are commercial products added to fluff pulps during sheet forming which make the pulp sheet softer and easier to fluff. Debonders are tlosely related 21 to fabric softeners chemically, and act in the same fashion. The force with which 22 pulp fibers bond is measured indirectly by measuring the force (or energy) 23 expended to debond or fluff a given pulp sheet.

24 The basis weiaht of a pulp sheet as described herein was determined on some of the products presented in the examples using a method 26 based on TAPPI T220. A sheet of pulp, commonly 30 cm x 30 cm or of another 1- convenient dimension, was weighed and then dried to determine the solids content 2 (%) O.D.). The area of the sheet was then determined and the ratio of O.D.
(oven 3 dried) weight to a defined area was reported as the basis weight.

4 The caliper and sheet densitv were determined on some of the products presented in the examples using a method based on TAPPI T220. Sheet 6 calliper was determined on test specimens from the basis weight test using a 7 motor driven micrometer that met TAPPI T411 conditions. Sheet density was 8 calculated as the ratio of basis weight to caliper.

9 Mullen strength and burst indexes were determined on some of the products presented in the examples using a method based on TAPPI T807. A TMI
11 Monitor Burst 1000T"" was used to measure the hydrostatic pressure required to 12 rupture (bursting strength) the pulp sheet when the pressure was increased at a 13 controlled constant rate through a rubber diaphragm to a circular area 30.5 mm 14 diameter. Mullen strength is recorded as kPa (kilo Pascals) at rupture, while burst index is the ratio of bursting strength to basis weight.

16 A KamasTM Lab hammermill Model H-01-C was used to defiberize 17 some of the products presented in the examples. Strips of pulp sheets 5 cm wide 18 were fed into the hammermill, using 900'rpm motor speed, 50% feeder speed, and 19 an 8 mm screen. In some cases, the energy required to defiberize the pulp sheet was recorded, and reported as W hr/kg of fluff, the energy of defiberization.
Fluff 21 was collected in a collection vacuum bag for further testing.

22 An M/K Formation Tester was used to measure the formation of 23 pulp sheets for some of the samples presented in the examples. The formation is 24 an expression of sheet uniformity. The M/K Formation Tester consists of a rotating glass drum containing a traveling light source. A pulp sheet is wrapped 26 around the outer surface of the drum. The light from inside the drum shines 1 through the sheet and strikes a detector outside the drum. During the test, the 2 drum rotates while the internal light source and the externai detector move 3 together down the axial length of the drum. In this way, the amount of light which 4 passes through the sheet is measured at several different locations. The variation in the amount of light which passes through the sheet from point to point on the 6 sheet is used as a measure of the formation (uniformity of formation) of the sheet.
7 Weighted average fiber length (WAFL) and fiber coarseness were 8 also measured for some of the products presented in the examples using a 9 KajaaniT"" FS-200 Fiber Analyzer.

1o Fiber Property Performance Tests ii SCAN testing of fluff puip properties was carried out on some of the products 12 presented in the examples. This test uses SCAN/PFI methodology (SCAN-C
13 33:80) and test equipment to form a uniform fluff sample, and to measure its 14 resiliency, fluid retention and rate of absorption. The fluff samples are conditioned for at least 2 hours under standard conditions (23 1 C and 50% 2% relative 16 humidity) prior to testing and are kept in the conditioning atmosphere throughout 17 the test.

18 A cylindrical fluff sample (3.00 0.05 g and 5 cm diameter) is 19 prepared using special equipment. The height of the cylinder under a 260 g/1.3 2 o kPa load is measured and reported as resiliency. The sample is placed in contact 21 with a water bath. The time required for the water to migrate vertically up the 22 cylinder to the top is reported as absorption time. The fluid retention or absorption 23 capacity per gram of sample is calculated by weighing the saturated fluff sample.
24 A fluff sample can also be subjected to simulated heat-aging artificially (105 C for two hours) and tested by this method to determine effects of 26 aging on fluff absorbent properties.

1 Dry classification of fluff pulp was carried out on some of the 2 products presented in the examples. This test is a measure of fluff quality and the 3 defiberization process. A JohnsonT"" Manufacturing Fluff Fiberization Measuring 4 Instrument, Model 9010, was used to separate the fluff into three fractions based on particle size. During the test, fluff is pneumatically agitated to separate the 6 fibers from each other and from the undefibered pulpsheet. A vacuum draws the 7 initial fines and then the long fibers through a rotating sieve screen (16 mesh, 1.18 8 mm opening, U.S.A. std. series). The initial fines also pass through a second 9 screen, and accumulate in a dust bag. The long fibers (accepts) accumulate on a second screen (45 mesh, 0.36 mm opening, U.S.A. std. series).
11 Pad integrity testing was carried out on some of the products 12 presented in the examples. Pad integrity is a measure of the strength of the fiber 13 network in fluffed pulps, and indicates how well the fluff will maintain pad integrity 14 in a dry formed absorbent product. The method is based on PFI method of 1981, "Measurement of Network Strength in Dry, Fluffed Pulps". During the test, a 16 cylindrical test pad of 1.0 0.05 gram and 50 mm diameter is prepared in a pad 17 former. The test pad is placed in a burst chamber, which is then installed in a 18 stress-strain apparatus. A burst-body is vertically forced through the test pad. The 19 force required to rupture the fiber network in the test pad is reported as pad integrity.

21 The potential of a fibrous pulp for use as an acquisition layer can be 22 described, among other tests, by a multiple "insult" or rewetting test. The Multiple 23 Insult - Absorption Testina procedure was carried out as follows. Pulps for 24 comparison purposes are fiberized, then airfiltered into pads with a basis weight of about 200 g/m2. The pads are pressed at 200 psig for a period of two minutes 26 then trimmed about 7 cm x 16 cm. The trimmed and densified pads are placed on WO 95l20066 ' ~ -~ 18 1163 PCT/US95100862 1 top of a standard absorbent core, such as a disposable diaper, and covered by a 2 single layer of conventional polypropylene coverstock. Fluid is introduced to the 3 absorbent product through a cylinder permanently mounted to a weighted plate 4 which applies a force of 0.1 psig to the absorbent product. A dam is used to control fluid flow to the absorbent product. A timer is started when the dam is 6 removed and fluid begins to move into the absorbent product. The timer stops 7 when all the fluid has been absorbed and the elapsed time recorded. Ninety 8 seconds after the fluid is completely absorbed a stack of five preweighed blotter 9 papers is placed on top and then a 1.0 psig load is applied to the absorbent product for a period of two minutes. The amount of fluid wetted back into the 11 blotter paper is recorded. The procedure is repeated two times for a total of three 12 wettings or insults". The multiple "insult" test characterizes the readiness with 13 which fibers absorb as well as reabsorbs a fluid.

AND EMBODIMENTS THEREOF

17 As mentioned above, it has now been found that various pulps of 18 diverse wood species prepared by diverse pulping and bleaching processes 19 provide improvements in these pulps by displaying improved fiber and pulp sheet properties, e.g. absorbency results such as for an acquisition layer in baby 21 diapers, etc. upon cold alkali extraction.(CAE) or cold caustic extraction (CCE) of 22 these pulps in the proper manner in the proper sequence when preparing these 23 pulps, i.e., when treating the pulps. Relatively high strengths of sodium hydroxide 24 solution are used ideally, 13% - 18% NaOH by weight for high absorbency, fast intensive absorbency applications and 5% to 15% for general absorbency 26 application, preferably 6% to 10% for that purpose. By "cold caustic extraction"
27 (CCE) is meant the treatment of pulp at a temperature less than 60 C, preferably 28 less than about 40 C, with the above sodium hydroxide solutions. The process WO 95120066 218t f63 PC'I'/US95/00862 1 coextensive with the preparation of the novel pulps is being claimed as an 2 improvement for the regime of the novel properties heretofore unrecognized in the 3 art. The improvement thus also resides in a method for improving, e.g., the 4 absorbency of the pulp, increasing the stiffness of fibers and other properties further described herein not heretofore known or recognized.

6 Moreover, it has been found as an embodiment that the appropriate 7 "acquisition layer' absorbency performance can be established after adequate 8 bleaching of high K number unbleached pulp has been carried out to obtain 9 aesthetically acceptable brightness values for the pulps with slightly lower cold caustic treatment (e.g. 15% NaOH versus 18% NaOH for unbleached pulps). At 11 the lower concentration of cold caustic solution bleached pulps are obtained which 12 are nearly as good as pulps obtained from CCE of the high K number unbleached 13 pulps themselves.

14 Accordingly, it has been found that a specific desirable pulp product regime exists based on the process employed and the selection of various product 16 or fiber criteria as will be further described herein. For example, the absorbency 17 relationships make the pulps in the characterized pulp product regime especially 18 useful because the pulps and their use can now be readily delineated from the 19 regime of unattractive uses ancl pulps not possessing the attractive characteristics.
Moreover, the relationships within this novel regime of other desirable properties 21 has been established so as to delineate with great precision the claimed regime of 22 the novel properties and the technique and process coextensive therewith.

23 Still further, while cold caustic treatment has been known for high 24 quality dissolving pulps as discussed above, e.g. to make alpha cellulose and some industrial product pulps, such treatment as correlated to the fiber and pulp 26 sheet property variables listed above is novel with respect to pulps useful such as 1 for absorbent pulps e.g. for an acquisition layer for products inter alia diapers, 2 incontinent and catamenial devices, etc. including absorbent core materials for 3 these.

4 Added and further benefits will appear from the following examples and the illustrative embodiments. The examples are merely for the purpose of 6 illustration and are not intended to limit the scope of the invention.
7 Example Improved Pulp Sheet Defiberization:
8 Debonders vs. Cold Alkali Extraction, Kraft 9 Southern Pine Pulp 11 Cellulosic pulp is commonly manufactured for fluff and other fibrous 12 end-use in dried, sheeted form. The pulp manufacturer operates the pulp machine 13 to form the sheet from an aqueous suspension of fibers; the sheet once formed is 14 dried to remove about 90% of the moisture. Large rolls of dried, sheeted pulp are produced off the dry end of the pulp machine. These are typically cut into smaller 16 size rolls and/or bales of sheets for distribution to end-use customers.

17 It is an advantage that the dried, sheeted pulp defibers easily and 18 uniformly without damage to the individual fibers for those pulp grades being used 19 in various fibrous end-use applications. For example, a fluff pulp will be converted by the end-user from the dried, sheeted pulp to a pad of "fluffed" fibers by 21 mechanical action such as is supplied by a hammermill or other attrition mill.
22 Chemical agents, debonders, are sometimes added to the pulp during sheet 23 formation to inhibit interfiber bonding, which results in softer, more easily defibered 24 sheets.

-15f - J

1 EXAMPLE 1, TABLE I-1 3 SAMPLE DESIGNATION A_1i B-ii Processing Non-debonded Debonded Standard Process Standard Process 6 Wood Species Southern pine blend . . . . . . . . . . . . . . . . . . >

8 Pulping Process Kraft . . . . . . . . . . . . . . . . . . . . . . . . . . .
. . . >

Sheet Debonder Used (?) No Yes 12 COLD ALKALI EXTRACTION Not Used Not Used ISO Brightness, % 88.5 89.4 18 Basis Wt. (g/m) 640 634 19 Caliper (mm) 1.36 1.36 Density (g/cm) 0.47 0.47 21 Mullen (kPa) 1113 417 22 Burst Index (kPas m2/g) 1.74 0.66 Resiliency (cm) 4.1 3.7 26 Fluid Retention (g/g) 13.4 11.4 27 Absorption Time (s) 28 Control 3.5 7.9 29 Heat-Aged 4.4 8.9 Dry Classification (wt. %) 31 Accepts 84.4 91.0 32 Knots 13.3 6.8 33 Fines 2.4 2.2 34 Pad Integrity (N) 7.2 7.0 WO95/20066 21Up1jU~3 PCT/US95/00862 1 f -16-1 EXAMPLE 1, TABLE II-1 3 SAMPLE DESIGNATION A=1ii B_1ii Processing Standard Process Cold Alkali (Non-debonded) Extraction Process 7 Wood Species Southern pine blend ----------------------------- >

9 Pulping Process Kraft---------- -->
11 Sheet Debonder Used (?) No No 13 COLD ALKALI EXTRACTION Not Used Used 14 Alkali Used NaOH
Solution Strength, % 7.5 16 Temperature, C 35 17 Time, H:M 10 18 Consistency, % 3 PULP ANALYTICAL PROPERTIES
21 ISO Brightness, % 88.6 89.6 24 Basis Wt. (g/m) 644 666 Caliper (mm) 1.12 1.17 26 Density (g/cm3) 0.57 0.57 27 Mullen (kPa) 1494 829 28 Burst Index (kPae m2/g) 2.32 1.25 KAMAS FLUFF CHARACTERISTICS
31 Resiliency (cm) 4.1 3.6 32 Fluid Retention (g/g) 12.9 13.2 33 Absorption Time (s) 34 Control 3.3 2.9 Heat-Aged 4.9 4.6 36 Dry Classification (wt. %) 37 Accepts 81.2 91.4 38 Knots 15.9 6.0 39 Fines 2.9 2.7 Pad Integrity (N) 7.2 7.4 WO 95/20066 21 C} f1J3 PCT/US95/00862 1 EXAMPLE 1, TABLE III-1 3 SAMPLE DESIGNATION A-liii B-liii -liii Processing Non-debonded Debonded Cold Alkali Standard Standard Extraction Process Process Process 6 Wood Species Southern pine blend------------------------------->

8 Pulping Process Kraft---------------------------------------------------->

Sheet Debonder Used (?) No Yes No 12 COLD ALKALI EXTRACTION Not Used Not Used Used 13 Alkali Used NaOH
14 Solution Strength, % 8.5 Temperature, 4C 35 16 Time, H:M 0:10 17 Consistency, % 3 1s ISO Brightness, % 86.6 88.4 88.9 23 Basis Wt. (g/m) 642 639 652 24 Caliper (mm) 1.36 1.30 1.33 Density (g/cm) 0.48 0.49 0.49 26 Mullen (kPa) 1126 716 770 27 Burst Index (kPa=m2/g) 1.75 1.12 1.18 Resiliency (cm) 4.1 3.9 3.6 31 Fluid Retention (g/g) 13.5 12.4 12.5 32 Absorption Time (s) 33 Control 3.3 7.1 2.5 34 Heat-Aged 4.3 7.7 3.0 Dry Classification (wt. %) 36 Accepts = 84.2 87.4 94.6 37 Knots ' 13.1 10.3 3.6 38 Fines 2.7 2.3 1.8 WO 95/20066 ~ 1 ( } ~
C~ I ~ , 3 PCT/US95/00862 1 Table I-1 of Example 1 compares some of the conventionally 2 prepared sheet property and fluff characteristics of "non-debonded" bleached 3 kraft Southern pine pulp (Sample " to debonded (with chemical debonder 4 added) bleached kraft Southern pine pulp (Sample B-1 i. The pulp sheet products were produced on a commercial pulp machine. The sheet properties (or sheet 6 physics) as well as characteristics of the fluffed fiber were tested as produced by a 7 small scale hammermill. The data given are averages of several tests on pulp from 8 several production runs. A description of the terms and tests has been given 9 above.

In comparison to the standard process non-debonded, sheeted 11 pulp, the standard process debonded sheeted pulp is softer (weaker) indicated by 12 the substantially lower pulp sheet Mullen strength as well as by the lower burst 13 Index. Note that the characteristics of the fluff from the debonded pulp are poorer 14 as indicated by the lower resiliency, lower fluid retention, and increased (slower) absorption times compared to those of the standard pulp fluff. The dry 16 classification data of the fluffed fibers from the debonded pulp do indicate, 17 however, that better or more uniform defiberization was achieved (higher accepts, 18 lower knots). The fluff pad integrity was equivalent for both types of pulp.

19 In Table II-1 of Example 1, pulp produced by the process of this invention, cold alkali extraction (Sample -1 ii is compared to standard process 21 pulp (Sample 6-1 ii . Both types of pulp were pulped by the kraft process from a 22 Southern pine chip furnish and were bleached to similar brightness using standard 23 chemicals/conditions of chlorine, chlorine dioxide, sodium hydroxide and sodium 24 hypochlorite. The data given are mean data for several samples tested during standard production and trial production periods. The conditions used during the = WO 95120066 2181163 PCTfUS95/00862 1 cold alkali extraction averaged about 7.5% NaOH solution strength, at about 2 for about 10 minutes at a pulp consistency of about 3%.

3 Note that the cold alkali extraction processed pulp sheet was softer 4 (about 45% lower in Mullen strength and in burst index) compared to the standard process pulp sheet. Also, the clry classification data of the fluff produced upon 6 small scale fluffing showed improvements in the greater percent accepts and in the 7 percent lower "knots" which indicates improved defiberability relative to the 8 standard process pulp sheet. In these respects, the effect of the cold alkali 9 extraction process on the pulp and fluff properties relative to the standard, non-debonded pulp were similar to the effects of the use of a chemical pulp sheet 11 debonder relative to standard process pulp (Table I-1, Example 1) and, in fact, the 12 novel pulps showed improved absorption properties. However, the cold alkali 13 extraction process did not result in any negative consequences on fluff absorption 14 times as does the use of a debonder. The fluid retention of the fluff from the cold alkali extraction processed pulp was equivalent to that of the standard pulp (Table 16 II-1, Samples A_iii and B-tii .

17 Note that the percentage improvement was greater in the weight 18 percent accepts (and in lower knot content) in the fluff from the cold alkali 19 extraction process pulp compared to the fluff from standard pulp (Table II-1) than the comparable improvement associated with the use of a sheet debonder (Table 21 I-1). The dry classification accepts were 12% greater and the knots 62%
reduced 22 for the cold alkali extraction process pulp relative to its control standard process 23 pulp, whereas accepts for the debonded pulp were increased by only 8% with knot 24 content reduced only 49% relative to its standard process control pulp.
Also, these relative improvements were achieved by the cold alkali extraction processed 26 pulp from a sheet that was actually somewhat harder than the debonded pulp 1. sheet (829 Mullen strength/1.25 burst index vs. 417 Mullen strength/0.66 burst 2 index).

3 The data presented in Table III-1, of Example 1 compare mill 4 production of both debonded and non-debonded standard pulps with trial production of cold alkali extraction pulp. All pulp types (Samples A-iiii, B-iiii, and 6 C-1 iii) were produced from a Southern pine chip blend furnish by the kraft pulping 7 process. All pulp types were bleached with chlorine dioxide, sodium hydroxide, 8 oxygen and/or hydrogen peroxide to the brightness level indicated. The cold 9 alkali extraction conditions achieved averaged about 8.5% NaOH solution strength, at about 350C for about 10 minutes applied to a pulp slurry at 3% consistency.

11 About 0.2% H202 (O.D. --oven dried-- pulp basis) had been added during the cold 12 alkali extraction.

13 Note that the debonded pulp and the cold alkali extracted pulp 14 sheet were produced at approximately the same Mullen strength and burst index, with both of these indicators of sheet hardness being substantially reduced for 16 either type of treated pulp, debonded or cold alkali extracted relative to the 17 standard process control. Again, the fluff properties for the cold alkali extracted 18 pulp showed some similarities to the debonded standard process pulp:
resiliency 19 and fluid retention were directionally lower for both relative to the standard pulp fluff. But the absorption times for fluff from the cold alkali extracted pulp were 21 better (faster) than for fluff from the debonded pulp or the standard process pulp.
22 Fluff dry classification weight percentage accepts and percentage knots were 23 directionally better for fluff from the trial cold alkali extraction pulp.

24 Thus, the use of cold alkali extraction resulted in advantages not found with the standard process pulp and/or not expected from known technology WO 95/20066 21811" 3 PCT/US95100862 1 of applying sheet debonders to standard process pulp as a means of "softening"
2 the pulp sheet.

3 Exam IR e 2. Cold Alkali Extraction for Fiber Property 4 IrTiprovement, Prehydrolyzed Kraft Southern Pine Pulp 6 The data presen'ted in-Tables 1-2 and 11-2 of Example 2 illustrate the 7 pulp sheet and fiber property irnprovements which occurred when cold alkali 8 extraction was appiied to pulps cooked from a Southern pine furnish by a 9 prehydrolyzed kraft process. The prehydrolyzed kraft process is a two-stage pulping process, in which the raw material furnish is treated first under a mildly 11 acidic condition (pH of about 3-4), followed by an alkaline stage which is basically 12 the kraft cook illustrated in Example 1.

WO 95120066 2181163 PCT/US95l00862 1 EXAMPLE 2, TABLE 1-2 2 SAMPLE DESIGNATION A_2i B=2i Processing Non-debonded Cold Alkali Standard Process Extraction Process 7 Wood Species Sou[hern pine blend >

9 Pulping Process Prehydrolyzed kraft -11 Sheet Debonded Used (?) No No 13 COLD ALKALI EXTRACTION Not Used Used 14 Alkali Used NaOH
Solution Strength, % 15 16 Temperature, 9C 25 17 Time, H:M 0:10 18 Consistency, % 3 ISO Brightness, % 89.4 86.7 22 Basis Wt. (g/m2) 652 818 23 Caliper (mm) 1.32 1.28 24 Density (g/cm3) 0.50 0.64 Mullen (kPa) 1154 716 26 Burst Index (kPa.m2/g) 1.77 0.88 28 Resiliency (cm) 3.8 4.0 29 Fluid Retention (g/g) 13.2 13.1 Absorption Time (s) 31 Control 3.4 3.4 32 Heat-Aged 4.2 6.1 33 Dry Classification (wt. %) 34 Accepts 95.0 97.3 Knots 1.8 0.7 36 Fines 3.2 2.0 37 Pad Integrity (N) 6.8 7.3 39 Absorption times, seconds 1st insult 4.3 3.1 41 2nd insuft 30.6 23.1 42 3rd insuR 45.1 31.1 WO 95/20066 218~ 16,3 PCT/US95/00862 1 DCAMPLE 2, TABLE 11-2 2 SAMPLE DESIGNATION A- ii B=24 Processing Non-debonded Cold Alkali Standard Process Extraction Process 7 Wood Species Southem pine blend >

9 Pulping Process Prehydrolyzed kraft >
11 Sheet Debonded Used (?) No No 13 COLD ALKALI EXTRACTION Not Used Used 14 Alkali Used NaOH
Solution Strength, % 10 16 Temperature, C 25 17 Time, H:M 0:10 18 Consistency, % 3 PULP ANALYTICAL PROPERTIES
21 ISO Brightness, % 90.5 87.2 24 Basis Wt. (g/m2) 847 897 Caliper (mm) 1.05 1.16 26 Density (g/cm) 0.81 0.77 27 Mullen (kPa) 1090 671 28 Burst Index (kPa=m2/g) 1.29 0.75 29 Kamas Energy (wh/kg) 116 83 32 Resiliency (cm) 3.8 3.7 33 Fluid Retention (g/g) 14.1 13.9 34 Absorption Time (s) Control 4.2 3.8 36 Heat-Aged 5.6 5.1 37 Dry Classification (wt. %) 38 Accepts 95.3 95.4 39 Knots 1.1 1.4 Fines 3.6 3.2 41 Pad IMegrity (N) 8.1 6.1 WO 95/20066 218116,3 PCT/US95/00862 1 Sample A-2i in Table 1-2 is a prehydrolyzed kraft Southern pine pulp 2 bleached with the conventional bleaching agents of chlorine, chlorine dioxide, 3 hypochlorite and/or hydrogen peroxide and/or oxygen and sodium hydroxide to 4 the ISO Brightness level indicated. Sample B-i 2in Table 1-2 is a similarly prehydrolyzed kraft pulp, similarly bleached to the brightness indicated prior to 6 cold alkali extraction.

7 The B=2i sample's processing included the cold alkali extraction a process under the conditions listed (average conditions used). Both the P 2i and 9 @2i samples were produced in a mill scale facility during production and trial runs, respectively.

11 As for the bleached Southern pine kraft pulp discussed in Example 12 1, the use of cold alkali extraction resulted in a softer pulp sheet (i.e., of lower 13 Mullen strength and lower burst index). Note that the higher basis weight and 14 density at which the -?i sample pulp was produced should have had a negative impact on these sheet properties. In addition, the resiliency and fluid retention of 16 the cold alkali extracted Sample -2i were equivalent to those of Sample A-2i and 17 the dry fluff classification results showed some improvement for Sample B-Z.

18 Kamas fluff absorption times were similar (slightly longer for Sample B-2i upon 19 heat-aging), but the specialized multiple insult absorption tests (described above) showed that cold alkali extraction improved the absorption properties of the 21 resulting fiber.

22 The data presented in Table 11-2 also compare bieached 23 prehydrolyzed kraft Southern pine pulps (pulping conditions were more severe 24 than those used for the samples in Table 1-2 of this example).

Sample A=2ii was produced without, Sample 6=2ii with cold alkali 26 extraction. Both types were also produced in a mill-scale facility and used WO 95/20066 2181163 PC I'/US95/00862 1. common bleaching techniques to reach the brightness levels indicated. The 2 sodium hydroxide solution strerigth used was lower than that used for the samples 3 described in Table 1-2 of this example, 10% vs. 15%.

4 Comparison of sheet property data again shows the sheet softening effects resulting from the use ol cold alkali extraction: lower Mullen strength, lower 6 burst index. Also, a Kamas energy parameter (see description above) was 7 recorded to describe the relative ease of defibering the pulp sheet during the 8 fluffing operation in the laboratory. The cold alkali extracted pulp was fluffed more 9 easily (with less energy input). Fluff absorptions were slightly faster for the cold caustic extracted Sample B=2ii. Dry classification of the fluffed fibers were 11 equivalent for both samples as were resiliency and fluid retention.
However, fluff 12 pad integrity (see description above) was poorer for the cold caustic extracted 13 Sample B(this was not the case with Sample 8=2ii compared to Sample A_2i in 14 Table 1-2 of this example).

Exam IR e 3. Cold Alkali Extraction Process:
16 Variable Solution Strength 18 From the data given in Tables 1-3 through VI-3 of this example, it is 19 apparent that no one set of cold alkali extraction process conditions will result in exactly the same consequences on every type of pulp. Raw material/furnish used, 21 pulping process used, and the position of cold alkali extraction within a bleaching 22 sequence have consequences on what may be the optimum conditions for each 23 type of sample. Secondly, it appears that cold alkali extraction conditions can be 24 selected to enhance some of the fiber properties of the resulting pulp but at the expense of.others. Not all fibrous end-uses require improvements in the same 26 properties, thus this apparent versatility of cold alkali extraction conditions might 27 be used to tailor pulp fibers for various fibrous end-use products and/or 28 customers. These points will be discussed in this and subsequent examples.

WO95/20066 21Q1Y Fl 3 PCT/US95l00862 =

1 DCAMPLE 3, TABLE 1-3 3 SAMPLE DESIGNATION A-3i pal Processing Non-debonded Cold Alkali Standard process Extraction Process >

7 Wood Species Southem pine blend >

9 Pulping Process Kraft >
K Number, mL 18 >

12 COLD ALKALI EXTRACTION Not Used Used >
13 Alkali Used (Control) NaOH NaOH
14 Solution Strength, % 7 12 Temperature, C 35 35 16 Time, H:M 0:15 0:15 17 Consistency, % 3 3 ISO Brightness, % 83.3 92.2 91.4 23 Basis Wt. (g/m2) 725 737 691 24 Caliper (mm) 1.75 2.14 2.41 Density (g/cm3) 0.41 0.35 0.29 26 Mullen (kPa) 1179 527 70 27 Burst Index (kPa=mz/g) 1.63 0.72 0.10 Resiliency (cm) 3.8 3.9 3.7 31 Fluid Retention (g/g) 13.3 12.2 14.6 32 Absorption Time (s) 33 Control 3.7 2.9 3.9 34 Heat-Aged 4.3 3.6 4.1 Dry Classification (wt. %) 36 Accepts 97.5 98.5 89.0 37 Knots 1.2 0.1 8.6 38 Fines 1.3 1.4 2.4 39 Pad Integrity (N) 6.7 6.4 5.3 = WO 95120066 2 1t:,l 1j t,} 3 PCTIUS95/00862 1 D~'~AMPLE 3, TABLE 11-3 2 SAMPLE DESIGNATION A- ii ii ii 22 Processing Non-debonded Cold Alkali Extraction Process->
Standard Process 7 Wood Species Sourhem pine blend >

9 Pulping Process Kraft >
K Number, mL 16 >

12 COLD AlJG4U EXTRACTION
13 Alkali Used None (water) NaOH >
14 Solution Strength, % 0 3 7 14 Temperature, 4C 35 >
16 Time, H:M 0:10 >
17 Consistency, % 3 >

ISO Brightness, % 87.9 90.3 92.1 92.0 23 Basis Wt. (g/mz) 711 677 676 691 24 Caliper (mm) 1.87 2.03 2.06 2.79 Density (g/cm3) 0.38 0.34 0.33 0.26 26 Mullen (kPa) 1189 1005 501 83 27 Burst Index (kPa.m2/g) 1.67 1.48 0.75 0.12 28 Kamas Energy (wh/kg) 109.5 99 92.7 -KAMAS FLUFF CHARACTERISTICS
31 Resiliency (cm) 3.8 3.5 3.3 3.3 32 Fluid Retention (g/g) 11.8 11.3 11.2 13.2 33 Absorption Time (s) 34 Control 4.1 2.8 2.6 4.0 Dry Classification (wt. %) 36 Accepts 94.6 94.3 94.0 75.9 37 Knots 2.0 2.7 3.2 21.1 38 Fines 3.4 3.0 2.8 3.1 39 Pad Integrity (N) 7.4 6.4 5.7 4.2 WO 95/20066 2 ' " 1( 63 PCT/US95/00862 =

1 EXAMPLE 3, TABLE 111-3 3 SAMPLE DESIGNATION - iii iii Processing Cold Alkali Extraction Process >

7 Wood Species Southern pine blend >

9 Pulping Process Prehydrolyzed kraft >
K Number, mL 16 > 11 -13 Alkali Used Sodium hydroxide (NaOH) >
14 Solution Strength, % 7.0 11.0 13.1 15.1 18.2 Temperature, 2C 352C- >
16 Time, H:M 0:1.5 >
17 Consistency, % 3 > - -ISO Brightness, % 88.0 88.3 85.3 85.3 85.7 23 Absorption Times, seoonds 24 1st insu@ 7.6 6.6 6.8 6.2 6.5 2nd insu@ 37.6 26.2 25.1 21.8 22.4 26 3rd insult 56.6 44.9 36.5 35.0 33.0 = WO 95120066 2181163 PCT/US95/00862 1 LXAMPLE 3, TABLE IV-3 2 SAMPLE DESIGNATION ~ B iv iv D iv E- iv a Processing Unbleached Pulp Unbleached Pulp Before Cold Alkali After Cold Alkali Extraction Extraction >

7 Wood Species Sourhem pine blend >

9 Pulping Process Kraft >
K Number, mL 8.2 >

12 COLD ALKALI EXTRACTION Not Used Used >
13 Alkali Used (Control) NaOH >
14 Solution Strength, % 6 9 12 15 18 Temperature, 2C 30 C >
16 Time, H:M 0:15 >
17 Consistency, % 3.0 >

Absorption times, seconds 21 1st insu@ 8.9 8.2 6.7 7.5 7.4 8.3 22 2nd insult 43.8 43.7 30.7 32.8 29.6 31.7 23 3rd insuR 64.5 68.5 51.2 48.3 50.0 46.3 WO 95/20066 21811" 3 PCT/US9q _/00862 =

1 DCAMPLE 3, TABLE V-3 2 SAMPLE DESIGNATION A-3v 4 Processing Standard Process Cold Alkali (Non-debonded) Extraction Wood Species Southern pine blend > -- --6 K Number, mL 12.4 >
7 COLD ALKALI EXTRACTION Not Used Used 8 Alkali Used (Control) NaOH
9 Solution Strength 6 Temperature, 2C 28 11 Time, H:M 0:15 12 Consistency, % 3 14 ISO Brightness, % 84.8 84.8 SHEET PHYSICS
16 Basis Wt. (g/m2) 644 599 17 Caliper (mm) 1.33 1.40 18 Density (g/cm) 0.53 0.44 19 Mullen (kPa) 1656 834 Burst Index (kP.m2/g) 2.63 1.44 21 Kamas Energy (wh/kg) 69.5 47.9 23 Resiliency (cm) 4.1 3.7 24 Fluid Retention (g/g) 12.0 11.8 Absorption Time (s) 26 Control 3.2 2.9 27 Heat-Aged 4.6 4.5 28 Dry Classification (wt. %) 29 Accepts 86.6 88.7 Knots 11.8 9.3 31 Fines 1.6 1.9 32 Pad Integrity (N) 7.1 7.0 yr 3 PCTIUS95100862 WO 95/20066 21~?p11U

1 EXAMPLE 3, TABLE 1/13 2 SAMPLE DESIGNATION f1- 3vi 3vi ~- 3vi D- 3vi E- 3vi 4 Processing Standard Cold Alkali Extraction Process >
Process (non-debonded) 6 Wood Species Southern hardwood blend >
7 Pulping Process Krafl >
8 K Number, mL 11.0 >

Alkali Used None Sodium hydroxide >
(control) 11 Solution Strength, % - 9 12 15 18 12 Temperature, C 30 C >
13 Time, H:M 0:15 >
14 Consistency, % 3 >
PULP ANALYTICAL PROPERTIES
16 ISO Brightness, % 31.5 43.2 38.6 37.6 37.8 18 Resiliency (cm) 3.4 2.9 2.9 3.0 2.7 19 Fluid Retention (g/g) 12.5 12.2 13.0 13.2 12.6 Adsorption Time (s) 21 Control 6.2 4.5 4.0 4.3 3.8 22 Heat-Aged 12.9 8.1 9.3 7.1 6.5 23 Dry Classification (wt. %) 24 Accepts 93.2 .93.7 91.6 91.5 90.4 Knots 0.7 0.6 0.6 0.7 0.5 26 Fines 6.1 5.7 7.6 7.8 9.1 27 Pad Integrity (N) 3.6 4.4 4.1 4.3 4.1 29 Absorption times, seoonds 1st Insult 13.3 11.9 11.4 11.7 10.7 31 2nd Insult 55.3 46.1 46.8 45.8 45.9 32 3rd Insuft 96a 64.2 67.3 73.6 74.3 WO 95120066 -2 1 811 U J PCT/OS95/00862 =

1 The data given in Table 1-3 of this example cover laboratory 2 experiments on bleached Southern pine kraft pulp. All Samples A-3i through C-3i 3 were bleached to the brightness indicated with the common bleaching chemicals 4 of chlorine dioxide, hydrogen peroxide and sodium hydroxide. The cold alkali extracted Sample B-3i and -9i were additionally bleached with chlorine dioxide 6 subsequent to cold alkali extraction (this contributed to the higher brightness levels 7 of Samples B-i 3and Q. The NaOH solution strength used in the cold alkali 8 extraction of Sample -i was relatively low (7% compared to that used for Sample 9 -.i, 12%). These samples were sheeted (non-directional sheet on a laboratory sheet mold) and dried under the same standard conditions in the laboratory (but 11 dried without restraint unlike a commercial pulp machine) so that the changes in 12 pulp sheet and fiber/fluff properties measured reflect the cold alkali extraction 13 process alone. Thus for Sample -~f, cold alkali extraction resulted in fibers which 14 formed a sheet which was fluffed into fibers with the following properties relative to Sample A-3i (non-cold caustic extraction): similar basis weight, higher caliper, 16 lower density, lower Mullen strength and lower burst index; equivalent fluff 17 resiliency but reduced fluid retention, faster absorption times and somewhat 18 improved dry fluff classification profiles. For Sample -3i (cold caustic extracted at 19 12% NaOH solution strength) relative to Sample A-3i (non-cold caustic extracted) the comparison/contrast was as follows: slightly reduced basis weight, higher 21 caliper, lower density, much lower Mullen strength and burst index (very weak 22 sheet); equivalent fluff resiliency, higher fluff retention, similar Kamas fluff 23 absorption times, and poorer dry fluid classification profile. Thus, if an end-use 24 required a fiber of highest fluid retention, a higher caustic solution strength could be selected; to maximize accept fiber upon fluffing, a lower caustic strength would 26 be preferable.

= WO95/20066 21l7' p11Ed[3 PCT/US95/00862 1 In Table 11-3 of this Example 3, data are presented as additional data 2 on bleached Southern pine krait pulp, produced in the laboratory over a wider 3 range of cold alkali extraction solution strengths. All samples A- ii through - ii 4 were bleached with the common bleaching agents of chlorine, chlorine dioxide, hydrogen peroxide and oxygen (prior to cold alkali extraction) to the ISO

6 brightness levels indicated. Even at 3% NaOH solution strength, the pulp sheet 7 can be somewhat softened without any large negative consequences on fluff 8 products. However, cold caustic extraction at 14% NaOH solution strength appear 9 to result in a pulp sheet that was fluffed with apparent negative consequences on dry classification and resiliency with no advantage in absorption time but with a 11 slightly higher fluid retention.

12 Results from a similar series of bleached prehydrolyzed kraft 13 Southern pine pulps cold caustic extracted over a range of from 7 to 18%
NaOH
14 solution strength are presented in Table 111-3. All samples A- iii through E- iii were bleached with chlorine, chlorine dioxide, sodium hypochlorite and sodium 16 hydroxide prior to cold caustic extraction. The multiple insult absorption test 17 results indicate that little benefit would be gained by using NaOH solution strength 18 in the cold caustic extraction (under the temperature, time and consistency shown) 19 greater than about 13% for this type of pulp, and that absorption times improve (decrease) progressively when using a 7% to 13% caustic solution.

21 Similarly, data are given in Table IV-3 of this example which illustrate 22 a levelling off of improvement of absorption times with increasing cold alkali 23 extraction solution strengths (6-18%). Samples B-3iv through F- iv were all cold 24 alkali extracted from the starting material Sample A-3iv. No bleaching chemicals were used on any of the Samples A-3iv through F- iv. Sample A-3iv was a 26 Southern pine pulp cooked to very, very low K Number via a single stage 1 conventional kraft cook in the laboratory. Multiple insult absorption times of the 2 fluff fibers were improved with the use of a 9% NaOH solution strength with no 3 further benefit being seen above the 9% strength. Thus a similar trend toward a 4 levelling off of absorption times with increasing solution strength seen from application of cold alkali extraction was observed for this low K Number 6 unbleached kraft Southern pine pulp as had been observed for the bleached 7 prehydrolyzed kraft pulp sample series given in Table 111-3 of this example.
But the 8 level of the absorption times at which each type of pulp absorbed and the solution 9 strength at which the absorption time improved occurred differently with the type of pulp extracted.

11 For a very low K Number bleached kraft pulp, cold alkali extraction 12 at relatively low NaOH solution strength has many advantages other than faster 13 absorption times. Data are given in Table V-3 of this example which compare two 14 samples (A-3v without and B-3v with cold alkali extraction) of pulp pulped to 12.4 K
Number and bleached to 84.8% ISO Brightness. The cold caustic extraction 16 conditions used for Sample B-3y were a relatively low solution strength of 8%, at 17 289C for 15 minutes at a pulp consistency of 3%. This cold alkali extraction was 18 used prior to bleaching to the indicated brightness. Both types of pulp samples 19 (data averages given for L-,gy and D,U were bleached using chlorine dioxide, hydrogen peroxide and sodium hydroxide.

21 One of the largest drawbacks to pulping to low K Number by the 22 kraft process is the negative consequences on fiber properties that result from the 23 extensive pulping. Please compare the higher sheet Mullen strength and burst 24 index of Sample A-3v, Table V-3 to those of the samples in Tables 1-3 and 11-3 of this Example 3. When the processing used on the low K Number pulp included 26 cold,alkali extraction (Sample B-3v_, Table V-3), these disadvantages were i overcome. In addition, the fluff characteristics of fibers from the R-v sample low K
2 Number pulp were equivalent to or better than the A-3v low K Number pulp sample 3 (Table V-3, similar fluid retentiori, somewhat faster Kamas fluff absorption times 4 and somewhat improved dry fluff classification profile).

In Table VI-3 of this example, data are presented for a series of 6 unbleached kraft pulp cooked from a Southeastern United States blend of 7 hardwoods (gums, oaks, etc.) to a low (11.0) K Number. Cold caustic NaOH
8 solution strength was varied from 9 to 18% for Samples B- vi through E:Bv1;

9 Sample A- vi was the starting pulp prior to cold alkali extraction. No bleaching io chemicals were used on these samples. The 9% NaOH solution strength appears 11 to be optimum of the conditions studied for this type of pulp in the unbleached 12 state: Kamas fluff and multiple insult absorption times are basically constant at 9%
13 and higher solution strengths. Dry classification profile for the fluff deteriorate at 14 solution strengths at or above 12%. For this type of hardwood pulp, even lower NaOH strength might prove to be more desirable. Note that hardwood pulps do 16 not match softwood pulps in these types of fibrous property performance tests.
17 However, cold alkali extraction can be used to improve some of these fiber/fluff 18 properties to some extent for both types of furnishes.

19 Ecam I. Sulfite Pulps: Debonders; Cold Alkali Extraction Debonders can be used on sulfite process pulps as well as on kraft 21 pulps. Data are presented in T'able 1-4, Example 4 for commercially available 22 sulfite pulps. The pulping process used is acid sulfite (also known as acid 23 bisulfite); both pulps are bleached to the brightness indicated by common 24 bleaching agents such as chlorine, chlorine dioxide, hydrogen peroxide and sodium hydroxide. Data given are averaged from several tests of each type of 26 production, non-debonded (A ,@ and debonded B-4i .

1 DCAMPLE 4, TABLE 1-4 3 SAMPLE DESIGNATION A=4i ~L4j Processing Standard process Standard prooess non-debonded debonded 6 Wood Species Northwest U.S. softwood blend, predominandy Douglas fir 8 Pulping Process Sulfite >

Sheet Debonder Used (?) No Yes 12 COLD ALKALI EXTRACTION Not Used Not Used ISO Brightness, % 91.8 91.2 18 Basis Wt. (g/m2) 698 684 19 Caliper (mm) 1.25 1.34 Density (g/cm3) 0.56 0.51 21 Mullen (kPa) 479 279 22 Burst Index (kPa.m2/g) 0.69 0.41 23 Kamas Energy (wh/kg) 41.0 28.7 KAMAS FLUFF CHARACTERISTICS
26 Resiliency (cm) 3.7 3.6 27 Fluid Retention (g/g) 13.2 12.1 28 Absorption Time (s) 29 Control 11.8 6.3 Heat-Aged 43.6 6.0 31 Dry Classification (wt. %) 32 Accepts 77.9 87.5 33 Knots 16.0 7.1 34 Fines 6.1 5.4 Pad Integrity (N) 6.3 6.4 WO 95120066 21Q 9 163 PCT/US95l00862 1 DCAMPLE 4, TABLE II-4 2 SAMPLE DESIGNATION A_4ii 1341il ii Dtii 4 Processing Standard Process Standard Process Cold Alkali Cold Alkali (non-debonded) (non-debonded) Extraction Extraction Unbleached Bleached Prooess Process Unbleached Bleached 6 Wood Species Sotahem pine blend >

8 Pulping Process Acid sulfite >
9 K Number, mL 34 28 34 28 11 COLD ALKAU EXTRACTION Not Used Not Used Used Used 12 Alkali Used NaOH NaOH
13 Solution Strength, % 15 15 14 Temperature, C 30 30 Time, H:M 0:15 0:15 16 Consistency, % 3 3 19 ISO Brightness, % - 86 - 86 22 Absorption times, seconds 23 1st insult 13:2 7.9 6.8 8.1 24 2nd insuft 36:3 372 20.9 27.3 3rd insult 45.1 63.5 30.1 38.6 WO 95120066 21 v ! 163 PCT/US95/00862 EXAMPLE 4, TABLE II{-4 3 SAMPLE DESIGNATION A-4iii - -4iii - - -Processing Standard Cold Alkali Processing Extraction (non-debonded) Process 6 Wood Species Caribbean pine 8 Pulping Process Sulfde > - 9 K Number 2: > - -11 COLD ALKALI EXTRACTION Not Used Used 12 Alkali Used Not Used NaOH
13 Solution Strength, % 15.4 14 Temperature, 9C 30 Time, H:M 0:37 16 Consistency, % 8 19 ISO Brightness, % 87.8 77.5 22 Resiliency (cm) 3.4 2.9 23 Fluid Retention (g/g) 12.1 13.0 24 Absorption Times (s) Control 2.8 3.5 26 Heat-Aged 4.4 4-4 27 Dry Classification (wt. %) 28 Accepts 92-4 80.4 29 Knots 1.6 11.3 Fines 6.0 8.3 33 Absorption Times, seconds 34 1st insu@ 38.1 15.9 2nd insult 88.2 45.0 36 3rd insult 135.8 69.6 = WO 95/20066 218116 3 PCT/US95100862 1 DGAMPLE 4, TABLE IV-4 3 SAMPLE DESIGNATION A-4iv B-4iv 6 Prooessing Standard Cold Alkali Process Extraction (non-debonded) 8 Wood Species Douglas fir >

Pulping Process Sulfit >
11 K Number, mL 26.6 >

13 COLD ALKALI EXTRACTION Not Used Used 14 Alkali Used NaOH
Solution Strength, % 15.4 16 Temperature, C 30 17 Time, H:M 1:00 18 Consistency, % 13 PULP ANALYTICAL PROPERTIES
21 ISO Brightness, % 90.4 83.4 23 KAMAS FLUFF CHARACTERISirICS
24 Resiliency (cm) 3.5 2.5 Fluid Retention (g/g) 14.1 13.0 26 Absorption Time (s) 27 Control 4.6 3.8 28 Heat-Aged 6.2 4.5 29 Dry Classification (wt. %) Aooepts 87.8 65.4 31 Knots 6.6 26.6 32 Fines 5.6 8.0 Absorption times, seconds 36 tst insult 47.2 28.9 37 2nd insu@ 103.3 59.9 38 3rd insufi 137.9 77.2 =

1 As in the Example 1, Table 1-1, which illustrated the effects of 2 debonders on bleached kraft pulp sheet properties, debonders can act to "soften"
3 the softwood sulfite sheet. Note the lower Mullen strength, burst index and Kamas 4 energy of Sampie 341 compared to Sample A_4i. There is also a similar trend toward lower fluid retention for the debonded pulp as was seen with the kraft pulp.
6 The dry fluff classffication profile is improved toward greater accepts, lower knots 7 as was the case with the kraft pulp. However, sulfite pulps differ from kraft pulps 8 in that the use of debonders improve absorption times for sulfite pulps (related to 9 the differences in wood derived extractives in acid sulfite pulps). Note the long fluff absorption times for the non-debonded sulfite pulp.

11 However, for sulfite pulps the use of cold alkali extraction can have 12 additional advantages and can improve performance in the multiple insult test.

13 Data are given in Table 11-4 of this example which compare multiple insult tests for 14 unbleached vs. bleached sulfite Southern pine pulps, processed with and without cold alkali extraction. Samples -4ii and 2:g were bleached with common 16 bleaching agents such as chlorine, chlorine dioxide, hydrogen peroxide and 17 sodium hydroxide. Samples A4ii and -4ii represent two high K Number 18 unbleached Southern pine sulfite pulps. Sample -4ii was cold alkali extracted 19 using the conditions indicated in Table 11-4 from Sample A-41i; Sample D_4ii was cold alkali extracted from Sample B-4ii.

21 These data indicate that cold alkali extraction can minimize 22 differences in multiple insult performance of these Southern pine sulfite pulps 23 apparent for unbleached vs. bleached pulp. Please compare the delta (A) for first 24 absorption times for to B-4ii of 5.3 seconds, but for delta first absorption times for D-4ii to C-4ii of 1.3 seconds; delta for third absorption times for B-9 to 26 A'i of 18.4 seconds, but only a delta of 8.5 seconds for the third absorption = WO 95120066 2181163 PCT/US95l00862 1 times for D-4ii to 0Thus cold alkali extraction reduced the magnitudes of the 2 differences in absorption times between unbleached and bleached pulps as well as 3 improving the actual level at which both cold caustic extracted samples Q
and D

4 performed (reduced all absorption times, further discussion of these samples is given in Example 5).

6 Data are presented in Tables 111-4 and IV-4 of Example 4 for sulfite 7 pulps which demonstrate the effects of using relatively high sodium hydroxide 8 solution strengths for cold alkali extraction over longer retention time and at higher 9 consistency than were used in the previous examples and tables. All four pulp samples A-4iii and B-4iii, Table III, A-4iv and B-4iv, Table IVj were bleached using 11 the common pulp bleaching chemicals of chlorine dioxide, hydrogen peroxide and 12 sodium hydroxide. Acid sulfite pulping was used to cook a Caribbean pine chip 13 furnish to 24 K Number (Table 111-4); acid sulfite pulping was used to cook Douglas 14 fir to about 27 K Number (Table IV-4). When cold alkali extraction was used (for the B samples of both these tables, i.e., B-4iii and B-4iv), it followed an initial 16 bleaching stage treatment of the unbleached pulp with chlorine dioxide.
Bleaching 17 was continued following the cold alkali extraction to the brightness level indicated 18 using chlorine dioxide, hydrogen peroxide and sodium hydroxide.

19 For the sulfite Caribbean pine pulp, the use of cold alkali extraction at 15.4% NaOH under the conditions listed resulted in fibers showing significant 21 improvement in the multiple insult absorption test times (all three insult times were 22 reduced about 50%). Kamas fluff characteristics were similar for the B-4iii sample 23 compared to the A-4iii sample with the exception of a poorer dry classification 24 profile for the cold caustic extracted sample B-4iii . This may be due to in optimally high NaOH solution strength for this type of pulp as was observed for 26 some types of kraft pulps discussed under Example 4, and/or the higher 1 consistency and/or longer time at which the relatively high concentration was used 2 could be non-optimum.

3 For the sulfite Douglas fir pulp of Table IV-4, the use of cold alkali 4 extraction also markedly improved the multiple insult absorption test times;
Kamas fluff absorption times were also faster but fluff resiliency and fluid retention 6 appeared to be more greatly affected for Caribbean pine of Table 111-4. The fluff 7 dry classification profile was also poorer with cold alkali extraction of this Douglas s fir sulfite pulp. Again, as with the sulfite Caribbean pine sample and with the kraft 9 pulp examples discussed in Example 4, these cold alkali extraction conditions may be non-optimum for fiber properties other than absorption time improvement for 11 this type of bleached sulfite softwood fiber.

12 Example 5. Kraft and Sulfite Southern Pine Pulps 13 The following unbleached kraft pulp (Sample -i - Table 1-5, 14 Example 5) with a K Number of 30 was obtained from a Southern pine chip furnish. This pulp was prepared by a routine conventional kraft pulping process 16 using methodology common to the industry. A sulfite process was used on a 17 Southern pine chip furnish to characterize the behavior of fibers pulped from the 18 same species via different pulping processes. This pulp was prepared by an acid 19 bisulfite process (sulfite process) common to the industry. This pulp (Sample A-5i - Table 1-5, Example 5) had a K Number of 34.

1 EXAMPLE 5, TABLE I-5 2 SAMPLE DESIGNATION A-5i D-Li Sc,S!

4 Processing Unbleached Pulp Unbleached Pulp Unbleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 6 Wood Species Sourhem pine blend >

8 Pulping Prooess Kraft >
9 K Number, mL 30 - -11 COLD ALKALI EXTRACTION Not Used Used Used 12 Alkali Used NaOH NaOH
13 Solution Strength, % 15 18 14 Temperature, C 30 30 Time, H:M 0:15 0:15 16 Consistency, % 3.0 3.0 19 ISO Brightness, % - - -22 Absorption times, seconds 23 1st insult 9.5 5.6 5.3 24 2nd insult 36.3 20.2 18.7 3rd insuR 56.9 32.4 26.7 1 DCAMPLE 5, TABLE II-5 3 SAMPLE DESIGNATION A- ii B= ii ii _ Processing Unbleached Pulp Pulp After Cold Pulp After Cold Before Cold Alkali Alkali Extraction Alkali Extraction Extraction 7 Wood Species Southern pine blend >

9 Pulping Process Sulfite K Number, mL 34 - -12 COLD ALKAU EXTRACTION Not Used Used Used 13 Alkali Used NaOH NaOH
14 Solution Strength, % 15 18 Temperature, pC 30 30 16 Time, H:M 0:15 0:15 17 Consistency, % 3.0 3.0 Absorption times, seconds 21 1sr insuR 13.2 6.9 5.1 22 2nd insult 36.3 24.5 18.6 23 3rd insuR 45.1 32.3 23.2 = WO 95/20066 ~ ,(~ I 1q63 PCT/US95/00862 -.{4~5-1 1 DCAMPLE 5, TABLE III-5 2 SAMPLE DESIGNATION A- iii - iii iii 4 Processing Bleached Pulp Bleached Pulp Bleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 6 Wood Species Sou[hern pine-blend >

8 Pulping Process Kraft >

COLD ALKALI EXTRACTION Not Used Used Used 11 Alkali Used NaOH NaOH
12 Solution Strength, % 15 18 13 Temperature, C 30 30 14 Time, H:M 0:15 0:15 Consistency, % 3.0 3.0 18 ISO Brightness, % 92 - -MULTIPLE INSULT ABSORPTION TEST
21 Absorption times, seconds 22 1st insu@ 8.9 5.5 6.4 23 2nd insu@ 41.6 18.8 23.1 24 3rd insuR 69.1 33.4 37.3 WO95/20066 2181163 PCT/US95/00862 =

1 Despite the different pulping processes, the Southern pine chip 2 furnish yielded fibers having excellent absorption results after cold alkali extraction 3 (Tables 1-5 and 11-5 or Example 5, the alkali used being sodium hydroxide).
Each 4 of the unbleached pulps was treated with a cold caustic solution of 15% and 18%
NaOH (weight%). The cold caustic extraction was carried out as follows. Pulps of 6 3% consistency [O.D. pulp weight/total weight (caustic solution + O.D. pulp) X

7 100] were treated at about 30 C for about 15 minutes by stirring the suspension.

8 For each different caustic solution treated sample, the absorbency was determined 9 and compared for the respective Kraft and sulfite pulp. It is noted that extraction with 18% NaOH gave the best test results for each of the pulp stocks.

11 For comparison, the unbleached kraft Southern pine pulp was 12 bleached to an ISO brightness of 92% prior to applying the cold alkali extraction 13 process (Sample A -iii Table III-5 Example 5). This pulp was the same pulp used 14 as the starting material for bleaching in Example 5 (Sample A-i, Table 1-5).

However, prior to cold caustic extraction it was bleached with the chemicals of 16 chlorine, chlorine dioxide, hydrogen peroxide, oxygen and sodium hydroxide.
The 17 results obtained are shown in Table III-5 when following the same cold caustic 18 extraction procedure as outlined above.

19 From the comparison of the data in Tables I-5 and 11-5 of this example, it is evident that for the unbleached pulp an increase in concentration of 21 the cold caustic solution to 18% NaOH improved the absorption properties;
for 22 bleached pulp (Sample A- iii, Table 111-5) the higher concentration (i.e., 18%

23 NaOH) reduced the absorbency properties compared to extraction with 15%

24 NaOH. However, note that the absorbency properties of the bleached pulp cold caustic extracted with 15% NaOH were distinctly better than those of the bleached 26 pulp processed without any cold alkali extraction.

= W O 95/20066 21~' 1 " 3 PCT/US95100862 1 Examale 6. Pn:hydrolyzed Kraft Bleached Southern Pine Pulp 2 In a manner simillar to that used for Example 5, the absorption 3 properties were determined for a bleached, prehydrolyzed kraft pulp from Southern 4 pine wood. This pulp was prepared by a routine prehydrolyzed kraft pulping process using methodology common to the industry and was bleached using the 6 chemicals of chlorine, chlorine dioxide, sodium hydroxide, and sodium 7 hypochlorite to an ISO Brightness of 86%. The K Number of the unbleached pulp 8 was about 18 mL.

WO 95/20066 2 163 PCT/US95/00862 =

1 EXAMPLE 6, TABLE 1-6 2 SAMPLE DESIGNATION A-&

4 Processing Bleached Pulp Bleached Pulp Bleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 6 Wood Species Southern pin >

8 Pulping Process Steam prehydrolyzed kraft >

COLD ALKALI EXTRACTION Not Used Used Used 11 Alkali Used NaOH NaOH
12 Solution Strength, % 15 18 13 Temperature, C 30 30 14 Time, H:M 0:15 0:15 Consistency, % 3.0 3.0 18 ISO Brightness, % 86 - -MULTIPLE INSULT ABSORPTION TEST
21 Absorption times, seconds 22 1st insult 6.7 4.9 6.2 23 2nd insu@ 46.6 19.6 25.5 24 3rd insult 77.2 32.3 41.9 25 i The absorption results after cold alkali extracting this pulp with 15%
2 and 18% NaOH are shown in Table I-6, and confirm the effect caused by CCE

3 treatment on the absorbency of the pulp. Again, this pine pulp subjected to 4 extraction after bleaching with 15% NaOH (Sample A-6j, Table I-6, Example 6) gave better results than that extracted with 18% NaOH.

6 In comparison to the absorption property data given in Example 5, 7 Tables 1-5 to 111-5, the absorption test results for the prehydrolyzed kraft Southern 8 pine fiber show that these are within a good range of absorbency despite having 9 been bleached to this relatively high brightness prior to cold alkali extraction.

Exam I~e 7. Kraft_Southern Pine Pulp: Unbleached K Number 11 Interaction 12 The accompanying Table 1-7, Example 7, illustrates a comparative series of 13 kraft Southern pine pulps where unbleached pulp K Number was varied (relative 14 severity of pulping - low K Nunibers indicate a more drastic pulping schedule with less lignin remaining in the pulp after pulping). In order to establish the desired 16 pulp property regime and pulping procedures, the bleaching of all three 17 unbleached stocks was carried out to equivalent brightness (92% ISO). The 18 bleaching chemicals of chlorine, chlorine dioxide, hydrogen peroxide, oxygen and 19 sodium hydroxide were used. It is noted that as unbleached K Number increased, resulting absorption properties after cold caustic extraction improved (lower 21 absorption times are better).

a_ A A n o y4;
u. a d ~ ~8 . . p O in _ '.-ma~~w z~c9or~s . .
v ::=

wl am~~ z - m maQd ~4 C p m cs , A
~ ~ maw = ~ 7z~~ioc~i Jp~ L m.-6 :A =. .
F= mars ;z w rn o ~ma~~~ ~Z'rceioo13 EL : =
~ =
0 o 'm at~ny ti~
~Z Z F omo a Z m n - W a y OZ O
p P
V o 8 w c ae Ja F~
Cl) wo, aa"m =1 ~'m w O MC pa ~ C5 ~.-J J ~~ G
N ~ J~ ~' 2 ~ 3 y~ ~a a ~ a ~

= J Y_ -~ C N QwJ T
H
fQCna dY OQCO F- r~ JQ C}
D co d ~ .
SUBSTITUTE SHEET (RULE 26) 1 Examole S. Sitka Spruce Sulfite Pulp 3 In a manner similar to that used for the Southern pine chip furnish, 4 spruce starting material was sulfite pulped. The sulfite process used was acid sulfite (also known as acid bisulfite) as in Example 5. The unbleached pulp was 6 subjected to cold caustic extraction. Data for the cold caustic extracted pulps 7 treated with 15% and 18% NaOH are shown in Table 1-8, Example B. It is noted 8 that while not all starting pulps perform at the same level, nevertheless there was a 9 significant improvement in absorbency after cold caustic solution treatment for each of the pulps obtained from this species. Both spruce pulp Samples B-81' and 11 Q-~ performed similarly (no significant difference between 15% NaOH and 18%
12 NaOH extractions).

SUE3STITUTE SHEET (RULE 26) WO 95/20066 21811" 3 PCTIUS95/00862 0 1 DCAMPLE 8, TABLE 1-8 3 SAMPLE DESIGNATION A4i - B-El Processing Unbleached Pulp Unbleached Pulp Unbleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 7 Wood Species Sitka Spruce . . . . . . . . . . . . - . . . . . . . . , . . .
. . . . . . __ . . >' 9 Pulping Process Sulfite . . . . . . . . . . . . . . . . . . . . . . . ... .
. . . . . . . . . . . . . _-. . . >, K Number,mL 31 .... ............................ ............. 11 12 COLD ALKALI EXTRACTION Not Used Used Used ~
13 Alkali Used NaOH NaOH i 14 Solution Strength, % 15 18 Temperature, QC 30 30 16 Time, H:M 0:15 0:15 17 Consistency, % - 3.0 3.0 ISO Brightness, % - -- -23 Absorption times, seconds 24 tst insu@ 70.0 12.2 10.0 2nd insult 43.7 223 24.1 26 3rd insuR 64.8 33.6 33.2 SUBSTITUTE SHEET (RULE 26) = WO 95120066 2l q ftP~11,U~3 PCT/US95/00862 ] Example 9. Western Hemlock Sulfite Pulp 3 This example illustrates the absorption properties obtained for a pulp 4 made from a western hemlock chip furnish by a sulfite pulping process (acid sulfite). Cold caustic extraction of the bleached hemlock pulp (ISO Brightness =

6 88%) again illustrates the improvement that results on cold alkali treatment: greater 7 speed of absorbency of fibers produced by cold caustic solution extraction.
The 8 data are given in Table 1-9, Example 9.

4MITUTE SHEET (RULE 2b~

WO95/20066 2181163 PCT/DS95/00862 =

1 EXAMPLE 9, TABLE 1-9 4 Processing Bleached Pulp Bleached Pulp Bleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 6 Wood Species Western Hemlock > ---9 Pulping Process Sulfite--- >
11 COLD ALKALI EXTRACTION Not Used Used Used 12 Alkali Used NaOH NaOH
13 Solution Strength, % 15 16 14 Temperature, C 30 30 Time, H:M 0:15 0:15 16 Consistency, % 3.0 3.0 19 ISO Brightness, % 88 - - -22 Absorption times, seconds 23 1st insu@ 12.3 7.7 9.4 24 2nd insuft 47.2 _ 31.9 39.9 3rd insul[ 75.1 44.7 62.0 SUBSTITUTE SHEET (RUI_E 26) 1 Example 10. BCTMP (bleached chemi-thermal mechanical pulp) 2 and Cold Alkali Extraction 4 In this example, BCTMP (a bleached chemi-thermal mechanical pulp) commercially available froim Tembec Co. was also extracted with 15% and 6 18% NaOH. The absorption test data (Table 1-10, Example 10) show substantial 7 improvement at the higher cold caustic solution strength. The K Number of this 8 BCTMP pulp was 36 mL. Even higher caustic solution strengths (e.g., about 20%) 9 may prove to be beneficial to absorbent property performance for fibers produced from this type of furnish via this pulping process. The wood furnish is a North 11 American, eastern Canadian softwood. Description of chemi-thermal mechanical 12 pulping and bleaching processes can be found in texts on pulping and bleaching.

SUBSTITUTE SHEET (RULE 26) 1 EXAMPLE 10, TABLE 1-10 3 SAMPLE DESIGNATION A=1Q B-t0i ~Q

Processing Bleached Pulp Unbleached Pulp Unbleached Pulp Before Cold Alkali After Cold Alkali After Cold Alkali Extraction Extraction Extraction 7 Wood Species Northern Softwood . . . . . . . . . . . . . . . . .. . . . >

9 Pulping Process Bleached Chemi-thermal mechanical . . . . . . . . . . . . .
. . . . . .. >
K Number, mL 36 . . . . . . . . . . . . . . . . . . . . . ... - . - - = = - -> - - -12 COLD ALKALI EXTRACTION Not Used Used Used 13 Alkali Used NaOH NaOH
14 Solution Strength, % 15 18 Temperature, C 30 30 16 Time, H:M 0:15 0:15 17 Consistency, % 3.0 3.0 ISO Brightness, % - -23 Absorption times, seconds 24 1st insult 9.7 8.8 4.0 2nd insult 39.8 37.8 25.1 26 3rd insult 61.2 59.8 35.4 SUBSTITUTE SHEET (RULE 26) = R'O 95120066 2181167a PCT/US95/00862 1 Example 11. Use of Cold Alkali Extraction on Semi-bleached, 2 Lower Brightness Pulp 4 The strength of caustic solution required to achieve optimum absorption properties is related to the type of raw material and to pulping and 6 bleaching steps used. In general, however, the less bleached (lower brightness) 7 the pulp, the higher the concentration of NaOH solution required to achieve 8 optimum properties. Also, the absorption properties attained are better when the 9 pulp is less bleached prior to application of a cold caustic treatment. This is illustrated below in Table I-11, Example 11, where two Southern pine kraft pulps 11 bleached to different brightness levels (ISO Brightness of 51 and 88, respectively) 12 underwent cold alkali extraction with 15 and 18% NaOH solutions. The results for 13 both of these pulps show that 15% NaOH gave the best overall absorption time 14 results (third insult time is the most significant one) with the pulp of lower brightness (semi-bleached pulp) yielding superior properties.
SUBSTITUTE SHEET (RULE 26) 1 DCAMPLE 11, TABLE I-11 2 SAMPLE DESIGNATION A-tti B-11i C-11i D-11i 4 Processing Semi-Bleached Pulp Bleached Pulp (ISO Brightness =51%)a (ISO Brightness=88%) After Cold Alkali Extraction-> After Cold Alkali Extraction-> 5 6 Wood Species Southern pine blend >

8 Pulping Process Kraft COLD ALKALI EXTRACTION Used Used Used Used 11 Alkali Used NaOH > - -12 Solution Strength, % 15 18 15 18 13 Temperature, C 30 30 30 30 14 Time, H:M 0:15 0:15 0:15 0:15 Consistency, % 3.0 3.0 3.0 3.0 18 Absorption times, seconds -19 1st insult 5.0 3.8 6.2 4.9 20 2nd insuR 22.1 21.2 22.2 24.8 21 3rd insuft 25.1 36.7 33.9 38.6 24 (a) Prepared by bleaching Sample A-11i of Example 11 (Table 11) with chlorine, chlorine dioxide, hydrogen peroxide, oxygen and sodium hydroxide to an ISO Brightness of 51.
26 (b) Prepared by bleaching Sample A-111 of Example 11 (Table 11) with chlorine, chlorine dioxide, 27 hydrogen peroxide, oxygen and sodium hydroxide to an ISO Brightness of 88.

SUBSTITUTE SHEET (RULE 261 1 EXAAAPLE 11, TABLE II-11 3 SAMPLE DESIGNATION A-11ii B-11ii ttii 1 ii Prooessing Semi-Bleached Pulp Semi-Bleached Pulp (ISO Brightness=38%)8 (ISO Brightness-44%) After Cold Alkali After Cold Alkali Extraction > Extraction >

7 Wood Species Southern pine blend >

9 Pulping Process Sulfrt >
11 COLD ALKAU EXTRACTION Used Used Used Used 12 Alkali Used NaOH > - - - - -13 Solution Strength, % 15 18 15 18 14 Temperature, 2C 30 >
Time, H:M 0:15 >
16 Consistency, % 3.0 >

19 Absorption times, seconds 1st insu@ 4.5 4.5 5.8 4.7 21 2nd insu@ 24.5 18.8 24.1 20.2 22 3rd insuR 36.4 30.2 41.1 31.2 23 (a) Prepared by bleaching Sample - ii of Example 5(Table 11-5) whh chlorine dioxide, 24 hydrogen peroxide and sodium Inydroxide.

WO95/20066 2 1 ~ ~ ~ ~ ~ PCT/US95/00862 SGt -60-1 All of the Samples A-11i through D-11i (Table I-11, Example 11) 2 were prepared by bleaching the 30 K Number Southern pine kraft pulp discussed 3 in Example 5(Sampie A-5i, Table 1-5) to the brightness level indicated, and then 4 cold caustic extracted under the conditions indicated. Note that in the unbleached state, 18% NaOH resulted in better absorption properties and that these absorption 6 times were better than those associated with semi-bleached pulps described in 7 Table I-11, Example 11.

8 When the 34 K Number unbleached Southern pine sulfite pulp of 9 Example 5, Table 11-5 (Sample A- ii was semi-bleached to ISO Brightness levels of 38 and 44, respectively, prior to cold caustic extraction with 15 and 18%
NaOH, 11 18% NaOH was still required to give optimum absorption properties. The results of 12 this work are seen in Table II-11, Example 11. Note that less bleached pulp (ISO
13 Brightness = 38%) still gives the best results when extracted with 18% NaOH

14 (Sample B-11 i' versus Sample -11 ii ; the results, however, are not as good as those observed by 18% NaOH extraction of the unbleached pulp itself with 18%
16 NaOH (see results for Sample - ii, Table 11-5, Example 5).

WO 95/20066 21U p d63 PCT/US95/00862 1 Example 12. Position of Cold Alkali Extraction 2 in a Multistage Bleach Sequence 4 The benefits of cold caustic extraction in improving absorbency occurs regardless of where it is applied in the bleaching sequence (e.g., at the 6 beginning, the middle, or at the very end). In the same multi-stage bleaching 7 sequence to prepare high brightness pulps there is even some indication that 8 when the same quantity of chemicals are used, there may be improved absorption 9 properties by applying the stage in the middle of the sequence. Such an example is now presented in which the ondy bleaching variable, in a 5-stage sequence to 11 prepare a fully bleached pulp frorn the same unbleached stock, was the position of 12 the CCE stage in the sequence; 15% NaOH solution strength was used.

WO 95/20066 2181163 PCT/US95l00862 1 EXAMPLE 12, TABLE 1-12 3 SAMPLE DESIGNATION A-12i B12i 12i.

6 Processing Fully Bleached Pulp Fully Bleached Pulp Fuliy Bleached Pulp, (5 Bleach Stages) with (5 Bleach Stages) (5 Bleach Stages) Cold Alkali w@h Cold Alkali wRh Cold Alkali Extraction in Stage 1 Extraction in Stage 3 Extraction in Stage 5 8 Wood Species Southern pin >

Pulping Process Prehydrolyzed kraft >
11 - _ 12 COLD ALKALI EXTRACTION Used >
13 Alkali Used NaOH >
14 Solution Strength, % 15 >
Temperature, C 30 >
16 Time, H:M 0:15 >
17 Consistency, % 3.0 > -ISO Brightness, % 84 87 84 23 Absorption times, seconds 24 1st insuft 17.7 14.4 19.2 2nd insuft 44.5 31.2 43.4 26 3rd insuH 67.7 57.2 70.4 29 The results shown above (Table 11-12) indicate that when CCE was used in the middle of the sequence (stage 3), the absorption time results were clearly 31 better (Sample B-12i than when CCE was used in the 1st or 5th stages. It was 32 interesting to note that ISO Brightness of the fully bleached pulp (Sample 33 was also improved relative to the other two (l.e., 87 versus 84%).

= WO 95120066 PCT/US95/00862 1 Exam f~. Kra1t Pulping Reject Material 2 In an effort to look at pulp that is even "rawer" or less pulped than 3 what normally occurs in conventional full chemical pulping processes, some 4 "knots" resulting from a conventional kraft cook of Southern pine chip furnish were cold caustic extracted with 18% NaOH. "Knots" essentially represent 6 pulping reject materials that are poorly cooked (relatively large in size unlike shives 7 and separable from the resulting pulped fibers via equipment loosely termed 8 "knotfers"). It was necessary to first defiber these knots in a Waring blender and 9 to flat screen this defibered material to remove reject material still remaining non-defibered prior to cold alkali extraction with 18% NaOH. The fibers had a very high 11 K Number (>50).

1 DCAMPLE 13, TABLE 1-13 3 SAMPLE DESIGNATION A=1$

Processing Defiberized Knots (Rejects) After Cold Alkali Extraction 7 Wood Species Southem pine blend 9 Pulping Process Kraft K Number, mL (80 mL test) >50 12 COLD ALKALI EXTRACTION Used 13 Alkali Used NaOH
14 Solution Strength, % 18 Temperature, 9C 30 16 Time, H:M 0:15 17 Consistency, % 3.0 ISO Brightness, % -23 Absorption times, seconds 24 1st insuB 5.4 2nd insu@ 13.9 26 3rd insuH 25.9 1 The multiple insult absorption test results shown in Table 1-13, 2 Example 13 indicate that these type of fibers after cold alkali extraction exhibit 3 good absorption times. The absorption times are equivalent to those of the cold 4 alkali extraction 30 K Number unbleached kraft Southern pine pulp (Sample Q-5i, Table 1-5, Example 5) and to those of the cold alkali extracted 34 K Number 6 unbleached Southern pine sulfite pulp (Sample Table 11-5, Example 5), 7 despite the raw material being essentially a waste material. A cold caustic 8 extraction would add significant value in turning this waste fiber into a viable 9 absorbent product.

It is believed that similar results would be obtained by stopping the 11 initial kraft pulping process at a point(s) corresponding to less delignification 12 overall and combining mechanical defiberization and screening steps prior to cold 13 alkali extraction and/or any bleaching desired to increase brightness (i.e., semi-14 chemical rather than full chemical pulping).

1. Example 14. Alkali Source Other Than Sodium Hydroxide:
2 Kraft White Liquor 4 A potential source of sodium hydroxide within a kraft pulp mill is white liquor used in the kraft pulping process. White liquor is a mixture of sodium 6 hydroxide and sodium sulfide. A suggestion is to carry out cold alkali extraction 7 using the alkaii present in white liquor (WL) as the source of NaOH; it is also 8 possible that the sodium sulfide present in the white liquor will have some positive 9 benefits. In Table 1-14, Example 14, are presented results of extraction of an io unbleached Southern pine kraft pulp with 9-18% NaOH in which some or almost all 11 of the NaOH requirements in the cold caustic extraction came from the white liquor 12 itself (the contribution of sodium sulfide to alkalinity was ignored). For comparative 13 purposes, cold caustic extractions with 9, 15 and 18% NaOH solutions were also 14 carried out as controls (Samples F-14i, G-14i, and H_14i, Table 1-14).

= WO 95/20066 2 181163 PCT/US95/00862 ~ x O m o z r ~Nm n O "_-'.

a~po ~O v~n rn mgn 'i V x sO~Ea > Cn ~
~ S z9 Sco tOrl: NOnJ
w !
T
-t ~OkE~ . ~ orn Z .~k~~ fC N c9 ~o t C J ~
at c5l Tc g E O ae E E n r~
w J E Z v.k (O N m ~'~
~Qt !
' ml C O.C o O? [7 N
J'WCy 001 N v .l.t'1 O~ m d) O z rn E
4I m m 0 ~
m Q~
3 oNn Tc 0 ~~ 'g at~w co z~? rm~
z O II
p O V
r ~ 32 ai za qJ X Jw C7V m E w ~ 2e Or ~ dY
m ~' . zi Z~
Z
o o ~' ~ a.~ ~ w.~y~wx wwN $ o3 ~x S~x aZi~
ax_ m~.~ yn~~c~'o?
~~d 3 a O~ ~irrcg 5 r c ~~

w m r-I N C7 d' ff1 t0 l- W Ol O c-I N M V' lf1 t0 [, CO 01 O ri N M V' rl .-f ~-1 rl ei H ri H ~1 Ii N N N N N

1 The use of white liquor to supply alkali was equivalent to the use of 2 sodium hydroxide at 15 and 18% NaOH solution strength (compare Samples 3 and G-14i, 0-14i and H-14i, Table 1-14, Example 14) in achieving improved 4 absorption properties relative to those of the non-cold alkali extracted unbleached Southern pine kraft pulp. At 9% solution strength, the use of white liquor appeared 6 to result in some improvement over the use of NaOH alone (compare Sample 7 14i to F-14i, Table 1-14i, Example 14). It is believed that at even lower alkali a solution strengths white liquor may also result in advantages over the use of 9 sodium hydroxide alone.

Example 15. Use of Hemi Caustic for Cold Alkali. Extraction 11 In using sodium hydroxide for cold alkali extraction, a caustic solution is 12 obtained which contains some organic material removed or "extracted" from the 13 pulp. This type of caustic solution is termed hemi caustic". The organic materials 14 solubilized during the cold alkali reaction with the pulp are considered to be predominantiy hemicellulosic materials (hemicelluloses are non-cellulosic 16 carbohydrate materials composed of xylose, mannose, or mixtures of these 17 monomers with glucose, etc. rather than the 100% glucose monomer of cellulose).
1s For a fibrous end-use pulp, cold alkali extraction may also remove some of these 19 hemicelluloses or other organics. However, the desired end-result is not chemically purer pulp fibers. Purity is required in dissolving pulps because these 21 pulps must function as chemical feedstocks in chemical end-use processes (esters 22 such as acetates, butyrates and nitrates, ethers, regenerated cellulose, etc.). For a 23 fibrous end-use application, the end result desired from the use of cold alkali 24 extraction is that the fibers produced exhibit improved performance as fibers -- as fluffed fibers in absorbent products, etc.; such appreciation of the desired end 26 result heretofore has not been recognized or known.

= WO 95120066 Z1Q11LlJ 1 Z PCT/US95/00862 v-69I-1 DCAMPLE 15, TABLE 1-15 3 SAMPLE DESIGNATION A"i5f B-15i 1 i 6 Processing Standard Cold Alkali Extraction Process (Bleached Pulp subsequent (Bleached Pulp to Cold Alkali Extraction->
prior to Cold Alkali Extraction) 8 Wood Species Southern pine blend >

Pulping Process Kraft >
11 K Number, mL 17.4 >

13 COLD ALKALI EXTRACTION Not Used Used >
14 Alkali Used (Control 100% 100% hemi NaOH caustic Solution Strength, % 15 >
16 Temperature, C 30 >
17 Time, H:M 0:15 >
18 Consistency, % 3 >

PULP ANALYTICAL PROPERTIES
21 ISO Brightness, % 84.4 85.5 84.4 24 Absorption times, seconds 1st insuft 4.7 4.9 4.9 26 2nd insuft 25.6 18.8 20.4 27 3rd insuft 44.8 29.9 36.6 1 The data presented in Example 15, Table I-15 show that hemi 2 caustic (i.e., caustic separated from the pulp after reaction under an initial pure 3 sodium hydroxide cold caustic extraction) can be reused to supply the alkali 4 source for subsequent cold caustic extractions for pulps with improvements in absorbency properties. Absorption times are improved relative to the non-cold 6 caustic extracted bleached Southern pine kraft pulp when the alkali source used 7 was either sodium hydroxide or hemi caustic. The hemi caustic solution used was 8 at 24.5% sodium hydroxide by weight and contained 2.9% "hemicellulose"

9 material.. The improvements when the hemi caustic was used were not as great as those when pure sodium hydroxide was used. However, it is expected that some 11 modification of the cold caustic extraction conditions (for example, increasing the 12 solution strength when hemi caustic is used) would make the effects of both types 13 of caustic equivalent.

14 It would also follow that other alkali sources when used in initially contacting the pulp in a cold alkali extraction could be reused in subsequent 16 extraction for these types of fibrous end-use non-dissolving pulps.

17 In the above Examples the cold caustic solution treatment or cold 18 caustic extraction of the pulp was typically at the indicated solution strength, at the 19 indicated consistency, for the indicated time at the indicated temperature, followed by a fresh water rinse, an acid wash (typically a sulfuric acid solution at pH
of 21 about 3) and a final fresh water rinse.

22 Other test data that were obtained also indicate that for the entire 23 range of concentration of the cold caustic solution, the concentration may range 24 between about 5% to 25% and higher but 13% to 18% gave the best results for the various pulp starting materials utilized for acquisition layers, i.e.
intensive, fast 26 absorption uses. A suitable concentration is dependent on the relative severity of 1 bleaching with the more severely bleached pulps requiring a milder treatment. For 2 absorbency improvements in general and also for improving yields and other fluff 3 pulp properties lower concentrations of caustic may be used i.e. to about 5%. The 4 versatility of the process has also been demonstrated for a variety of pulp source materials.

6 As illustrated in the examples above the cold caustic solution has 7 been a sodium hydroxide solution, but other alkali materials may be used.
Other 8 alkali materials such as potassium hydroxide etc. may be used but at a severe 9 economic penalty such that their use is prohibitive.

Ukewise, a combiriation of sodium hydroxide solution and a water 11 soluble, non-toxic glycol, (e.g., propylene glycol solution) might also be used, but 12 the added cost is less justified for this large volume bulk product.

13 In describing the regime for the acceptable starting pulps and 14 process conditions for CCE treatment, this regime may be characterized as follows: for fast absorbency improvements such as measured by the insult tests, 16 especially the third insult; the K Nlumber related to absorbency and severity of 17 pulping; the severity of pulping which may be avoided when practicing the present 18 utilization of various pulps in bleached and unbleached conditions;
enhanced 19 yields of accept fibers upon fluffing; advantageous use of reject materials; use of mill by-products; swing capability to insert in the bleaching treatment steps the 21 CCE step in any bleaching sequence; fluff pulp properties not requiring debonders, 22 i.e. without additives, etc. etc. Such improvements especially in combination with 23 each other have heretofore not been recognized, known or practiced for fluff pulps 24 and thus have not shown the way to the unique combination(s) of properties described above.

1 The basis weight of acquisition layers in current products ranges 2 from 75 to 200 g/m2. As an example, the acquisition layer 12 shown in Figure 2 is 3 an air laid fluff web of 200 g/m2. This web is separated from the absorbent core 4 13 by a layer of conventionally wet-laid tissue paper 13. The core may be wrapped in such tissue paper. The absorbent core is a mixture of cellulose fiber, 6 fluffed and airlaid with super absorbent polymer (SAP) available from commercial 7 sources. The basis weight is about 500-700 g/m2. There is a moisture proof 8 polymer backsheet 16 below the core of 0.5 mil. Wet laid sheets may also be 9 used.

The above described examples, embodiments, and comparisons are 11 intended to illustrate the various aspects of the invention without limitation of same 12 but the appended claims and elements thereof including reasonable equivalents 13 for these are to define the metes and bounds of the invention.

Claims (10)

Claims
1. ~An absorbent article comprising a fluffed alkali treated absorbent pulp which is without chemical crosslinking covered with a fluid permeable topsheet characterized in that the alkali treated absorbent pulp is produced by suspending a cellulosic pulp in an alkali solution of a concentration from 3%
to 25% by weight for a treatment time from five minutes to one hour at a temperature below 60°C, recovering the alkali treated pulp from the suspension, drying the alkali treated pulp and fluffing the dried alkali treated pulp.
2. ~The absorbent article of claim 1, wherein the treatment temperature is less than 40°C, the suspension has a consistency of from 2% to 10%, and the alkali solution has a concentration from 6% to 18% by weight.
3. ~The absorbent article of claim 2, wherein the alkali solution has a concentration from 13% and to 18% by weight.
4. ~The absorbent article of claim 3, wherein the suspension has a consistency from 3% to 8% by weight.
5. ~The absorbent article of claim 1, wherein the absorbent article is a baby diaper having a water barrier sheet, and said absorbent pulp is between said fluid permeable coversheet and said fluid barrier sheet.
6. ~The absorbent article of claim 1, wherein the absorbent article is a catamenial device.
7. ~The absorbent article of claim 1, wherein the absorbent article is an incontinence device.
8. The absorbent article of claim 4, wherein the absorbent article is a baby diaper having a water barrier sheet and the absorbent pulp is between said fluid permeable coversheet and said water barrier sheet.
9. The absorbent article of claim 4, wherein the absorbent article is a catamenial device.
10. The absorbent article of claim 4, wherein the absorbent article is an incontinence device.
CA002181163A 1994-01-21 1995-01-19 Cold caustic extraction of pulps for absorbent products Expired - Fee Related CA2181163C (en)