CA1055318A - Brazing aluminium - Google Patents

Brazing aluminium

Info

Publication number
CA1055318A
CA1055318A CA249,854A CA249854A CA1055318A CA 1055318 A CA1055318 A CA 1055318A CA 249854 A CA249854 A CA 249854A CA 1055318 A CA1055318 A CA 1055318A
Authority
CA
Canada
Prior art keywords
flux
brazing alloy
components
slurry
aluminium
Prior art date
Legal status (The legal status is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the status listed.)
Expired
Application number
CA249,854A
Other languages
French (fr)
Inventor
William E. Cooke
Current Assignee (The listed assignees may be inaccurate. Google has not performed a legal analysis and makes no representation or warranty as to the accuracy of the list.)
Alcan Research and Development Ltd
Original Assignee
Alcan Research and Development Ltd
Priority date (The priority date is an assumption and is not a legal conclusion. Google has not performed a legal analysis and makes no representation as to the accuracy of the date listed.)
Filing date
Publication date
Application filed by Alcan Research and Development Ltd filed Critical Alcan Research and Development Ltd
Application granted granted Critical
Publication of CA1055318A publication Critical patent/CA1055318A/en
Expired legal-status Critical Current

Abstract

ABSTRACT

A method of joining aluminium components by means of an aluminium brazing alloy having a melting point lower than that of the aluminium components, in which the assembled components are heated to a temper-ature above the melting point of the brazing alloy and below the melting point of said components in the presence of a potassium fluoaluminate flux, which is essentially free of unreacted KF characterised in that the flux and the brazing alloy is applied to the surface of at least one of the components as an aqueous slurry of finely divided flux and metal powder, the film is then dried and the components are brazed (after assembly, if necessary) by heating in a dry, oxygen-free inert gas atmosphere, the application of flux/brazing alloy slurry being controlled to apply 40-150 gms/m2 of solids And the flux:brazing alloy ratio being selected to deposit at least 5 gms/m2 of flux.

Description

1(~553~8 The present invention relates,to methods of joi~ing aluminium (including aluminium alloys) by,brazing~
It is already known to joi~ aluminiu~ components,by melting an aluminium brazi~g alloy between or adjacent the faying surfaces (i.e. the surfaces to be joined), in the presence of a flux, which dissolves or disrupts the aluminium oxide film on the metal surfaces, It is commonly preferred that the melting point of the brazing alloy be,at least about 30 to 40C lower than that of the metal of the components.
~n example of a suita~le brazing alloy is an Al-Si eutectic composition, which melts at about 577C and thus melts at a -~
temperature which is at least ~0C below the ~elti~g point of aluminium and most commonly-used alumi~ium alloys.
Although it is normal practice for at least one component to be made from brazing sheet (aluminium alloy clad with aluminium brazin~ alloy), it is also known to apply the bra~ing alloy as a powder, carried in a suitable liquid or pa~te-like vehicleO
' ~luxless aluminium brazing is knot~ which requires to be performed at sub-atmospheric pressure and is ther~fore expensi~e and inconvenient. Other fluxless methods, which re- ~ , quire the use of an inert àtmos?here at atmospheric pressure, ,~ ;
,,~re also Xno~m, but these are hi~hly sensitive to even trace amounts of oxygen and water vapour contamination of the at~os-phere and are likewise expensive and inconve~ient to operate.It is, thererore, normal practice to e~ploy a flux in brazing aluminium to remove the oxide filn ordinarily .
,,. ......... .,. .

` ~

531~

present on aluminium surfacesv The materinl used a~ a flux must be capable of dissolving or disrupting aluminium oxide at the brazin6 temperatures while remai~ing essentially inert with respect to aluminium at such temperatures.
It has been usual to employ mixtures of metal chlorides' as fluxes for brazin~ alumini~ hese fluxes are essentially water-soluble and usually hygroscopic and are corrosive to aluminium (including aluminium brazing alloys) in the presence of water; hence residues of such fluxes must be removed by washing at the end of the brazing operationO
It has already been proposed to use a mixture of a powdered brazing alloy with chloride flux in a suitable liquid vehicleO ~he required vehicle has thus been limited to organic liquids in which the chloride-containing flux does not attack the brazing alloy particles. ~ecause the fluxes are h~groscopic, this expedient has not been satisfactory, since it has been necessary to proceed with the brazing operatlon as soon 8s the vehicle had dried.
We have already described in C~dia~ ~pplication No~177~926 aluminium brazing fluxes consisting essentially of one or more potassium fluoalumi~ate complexes (either XAlF4 alone or iu admixture with K3AlF6) and essentially free of unreacted A potassium ~luoride. ~hese flu~es are non-hygroscopic a~d leave no substantially water-soluble residue. Such fluxes are reactive at ~emperatures above about 560C to strip from or dissolv~ ~xides on alu~iniu~ surfaces but are essentially ~`
i~ert with respect to metallic aluminlum so that there is ~o ~, .

,. .,~ , ;

. .

. i 1~553~1L8 necessity to wash a brazed assembly to remove flux residue for avoiding cor-~osion.
The present invention broadly contemplates the provision of an alum-inium brazing method wherein a mixture of powdered aluminium brazing alloy and a powdered potassium fluoalumina~e flux of the ~ype ment:ioned above are applied to or adjacent the faying surfaces of aluminium components in an aqueous vehi-cle, the components being ~hereafter appropriately heated in assembled relation so that the brazing alloy powder melts and forms a brazed joint. After heating, the components are cooled to solidify the join~.
Accordingly, the invention provides a method of joining aluminium com-ponents by means of an aluminium brazing alloy having a melting point lower than that of the aluminium components, in which the assembled components are heated to a temperature above the melting point of the brazing alloy and below the ;~
melting point of said components in tbe presence of a potassium fluoaluminate ~lux, which is essentially free of unreacted KF characterized in that the flux and the brazing alloy is applied to the surface of at least one of the compon-ents as an aqueous slurry of finely di~ided flux and metal powder, the film of slurry is then dried and the co~ponents are brazed ~after assembly, if necessary) ~ by heating in a dry, oxygen-free inert gas atmosphere, the application of
2~ flux/brazing alloy slurry being controlled to apply 30-180 gms/m of solids and the flux:brazing alloy ratio being selected to deposit at least 3.29 gms/m2 of flux.
Thus, we have now discovered that the said flux, consisting essenti-ally of potassium fluoaluminate possibly with some unreacted AlF3 but essenti-~ally free of unreacted potassium fluoride, may be maintained in an aqueous slurry with powdered aluminium brazing alloys for extended periods of time wlthout delete~iously attacking the brazing alloy particles. We have found, , ~ery surprisingly, that aluminium brazing alloy particles and flux particles ,3~
., .

1, '~ ' ` 10553~8 may be deposited on aluminium from such slurry and be drled to form a film which has reasonable adhesion to the alumlnium. By contrast~ a slurry of alu-minium brazing alloy partlcles alone does not rorm a fi]m of adequate adhesion.
In some circumstances as little as 2% flux in the total sollds of the sl~ry is sufflcient. More usually it ls preferred that the flux should be present in an amount of 10-20~ of the amount of the brazing alloy particles by weight.
The weight of water ln which the mixture of flux and metal powder is dispersed may be varled depending on the desired consistency of the dispersion, but is typlcally less than the weight of powder dispersed in it.
While the slurry may be applied by spraying or brushing, the most convenient procedure for high volume commercial production of brazed assemblles is to dip the components ~1tO the slurry before or after assembly. This leads to deposition of the slurry on all the available surfaces of the components.
Surface effects lead to preferential deposition between faying surfaces when assembled components are dipped. The particle size of the flux and metal pow-der should both be less than 200 mesh ~less than 75 microns) to ensure entry between the faying surfaceæ of assembled componenks.
By variation of the amount of water in the slurry and by control of other factors, particularly the rate of withdrawal of the component or assem-bly of components from the slurry, it is possible to deposit a slurry coatinghaving a solids content of 40-150 gms/m2. Such coating after the necessary drying step has sufficient adhesion to the aluminium component to allow it to be handled. It is, of course, necessary to pretreat the surface to ensure that the surface has been adequately degreased to allow the slurry to wet the sur-~ace.
Ihe thus deposited coatings of flux and brazing alloy powder may con-tain sufflcient flux to permit the brazing to -5- , .

- , ~' .

' 1C~5533 .
be carried out in the ~ormal oxidising atmosphere of a - brazin~ furnace~ ~owever, the quantity of flux required ~or such operation i5 50 high that large qua~tities of unsightly flux residue result and furthermore the costs ~f the brazing operation are si~nificantly increased. ~herefore, as a ~urther feature of tl~e invention the brazing operation is performed i~ a furnace havin~ an atmosphere of a dry - ;~
inert gas~ ~he atmosphere is commonly dry oxygèn-free`~
~itrogen, i.e. dried to a moisture content of less than 250 p.p.m. water vapour and having a free oxyge~ content of less thau ~000 p.p.m. Other gases, which are i~ert to alumi~ium, such as cr~cked ammonia, may be employed pro~-ided ~ ;
_" ~ ;
that their free oxygen and moisture content are held do~i~ to , the sRme levels. ~he fur~ace atmosphere is held at a temper~
ature above the melting point of the powdered aluMinium brazing alloy a~d of the flux, but below that of the aluminiu~
or aluminium alloy components, which are to be joined by the - brazing operation. ~his brazing procedure is satisfactcry , , ~ ~or almost all aluminium alloys which have a solidus te~per-; 20 ature above the liquidus temperature of the brazing alloy.
~owever, the flux provides less satisfactory results whe~ the components to be Joined (ox one of them) has a Mg content in excess of about 1~ -As already explained, the flux/brazing alloy ratio ~ ~ -of the slurry may be varied through quite wide li~its. It is, ~ ~
.' ~ ~ however, us~ally satisfactory to operate the process wit~ a ;; flux content of 5-15 gm/m2 i~ the dried film. ~hus the ratio :.; . . . .
,, ~ -6-,, r :~ . . .
'.

l~SS3~8 of powdered br~zing alloy filler metal ~nd water to flux will preferably be arranged so as to deposit a desired coating wei~ht of brazing alloy in conjunction with a flux content in the stated range. There is no upper li~it for the amount of flux from the point of view of ~or~ing a~ -effectiv~ joint. However the appearance of the work is marred by heavy fused ~lux residues and ther~fore it is preferred to restrict the flux to not more than 50 gms/m20 ~he powdered brazin~ allo~/flux slurry may incorporate suspension agents and corrosion inhibitors, but these do not appear to be necessary in a~y operation ~here `
the dwell time of the slurry in the bath is of limited duration. Small quantities of surface active agents m~y be included to assist in penetration of the slurry between the ~aying surfaces of an assembly.
~ he present process finds exceptional utility in the production of heat exchanger assemblies, such as oil coolers for motor vehicles.
; . , - ~, . . .
~ As already stated, the flux consists essentially of a mixture of potassium fluoaluminates, essentially free o~
unreacted potassium fluoride. As herein used, "potassiu~
fluoaluminate" refers to substances of the type f or~ed b~
~usion of AlP'3 and KF, such complexes having the formulae K3A1~6 and KAlF4. X-ray diffraction examination of the solidified residue of the fused eutectic mixture of ~F ~nd ~ -AlF3, which occurs at about 45.8% ~F and 54O2~ AlF3, indicates that virtually all the fluoriae co~tent-s are in --7-- ~ `

. . ,.,".~. .. ,.. ,, ~
! ~

;
... ... . . ~` . . .
,. . . .

1~5531~3 the form of K~Al~5 and KAlF4, which are very sparingly soluble in water and are non-hygroscopic. The fused eutectic consists of these two phases and is virtually free of ~F and AlF3-~he liquidus point of a mixture of potassium fluo-aluminates varies depending upon the co~position of the ;
mixture, expressed as relative proportions of AlF3 and ~F, reaching a minimum ~about 560C) at the aforementioned eutectic composition and it is accordin~ly preferred to e~plo~ -~
~0 a flux which complies closely with the eutectic composition.
~owever, other flux compositions within the broader composition limits stated in ou~ C~dian ~pplicatio~ ~o.l~6 in the process of the present invention. ~hile the flux . melting point shown in ~he published diagram (Journal American Ceramic 80ciety, 49, pa~es 631~34, December 1966) rises Yerv : rapidly if the ~uantity of ~F rises above that re~uirec~ for the eutectic, there is only a slight rise in ~elting point . to about 574C where the AlF3 rises above the eutectic up to a total of about 6~o (50 ~ole % AlF3). ~or aluminiu~
brazing operations, it is commonly preferred that the Al~
ratio of the potassium fluoalu~inate be such that the flu~
becomes reactive at not more tha~ a`bout 600C. ~referably, the flux îs an intimate mixture of K3A1~6 and ~h1~4 corres-. . .ponding to an AlF3fKF ratio between about 60:40 and about . 50:50, in parts ~.y weight, essentially free of unreacted ~.At compositions corresponding to ~n AlF3 content ~ below about 60~, the mixture of potassium fluoaluminate . .

,.,, , ,. ., ~
.. , . .

, ~ .

1~553~

complexes, in dry state, consists essentially of K3AlF6 and ~AlF4. At higher levels of A1~3 content within the stated range, the mixtures are constituted of KAl~'4 with some ; unreacted AlF3 (which is insoluble in water~ but, again, essentially free of unreacted KF. ~!inor a~ounts of otker fluorides (e.g. ~iF, Na~ or CaF2) may be incorporated in the fluxo , Because the potassium fluoaluminate flux does not ; deleteriously attack brazing alloy powder when mixed in water, the powdered flux-alloy bath has a useful life of ~everal days or longer, whereas the use of a conventional chloride flux in such a bath would have a short life o~irlg to attack on the brazing alloy by the chlorides~ Irldeed, it is found that a slurry in accordance with the present invention can be rejuvenated by a 1~ weight addition of the flux and brazing alloy powder in the desired proportions~
Various additions may be made to the aqueous slurry of *lux and brazing alloy powders without departing fro~ the present invention. For example~ conventional surfactc~nts, thickeners and/or dispersing a~ents may be employed. In practice, however, satisfactory results have been achieved without any of these additives.
~ ~IE I
. .
One hundred parts by weight of -200 ~esh size Al-1~1~ Si brazin~ ailo~ powder and 25 parts by weight of -200 mesh size potassiu~ fluoalur~nate powder (a ~ixture of ~hlF4 ~nd K3A1~6) were mixed with 75 parts by wei~ht cf de-io~ized , ' . , _9_ .

.~' . . . ~ .

. .

1a~553~

water and maintained in suspension in the resulti~g slurry by mechanical stlrring. Small specimens Or cleaned alumlnium, 2.5 cm x 2.5 cm, were dipped in the mechanically stirred ~
slurry and withdrawn at a rate such that a unifor~ deposi~
; 5 o~ flux and metal powder re~ained on th~ surfaces of the - ~pecimens. Aft~r drying, the coa~in~ of flux and brazin : alloy powder was removed from all but o~e surface of each ~pecimen. Coating weights ranging from 30 to 1~0 grams per ~quare metre were produced in this way, merel~ by varyin~ ~he consistency o~ the slurry by dilution with water. Each speci-men was successfully brazed to an u~coated specimen in a tube fur~ace having an atmosphere of dry nitrogen.
EXA~E II
A slurry ~las prepared consisting of 4 gra~s of the potassium fluoaluminate flux powder, 160 grams of the ~l-Si brazing alloy powderl and 108 ml, of de-ionized water. This slurry was applied to surfaces of aluminium samples so as to ,; .
achieve a coating weight (after drying) of 135 grams per square metre. Fully effective brazing was achieved with the 20 samples thus coated, althou~h the metal/fluY ratio in this instance was 40~
; EXAMEIE lII
~ slurry consisting of 10 parts Al-1a~o Si brazi~-alloy powder and 1 part of flux (the eutectic mixture of RAlF4 and K3hlF6) was mixed with su~ficient water to provide, after immersion of plates of aluminium alloy ~esignated ~A3003 intended to form an oil cooler heat eY~ha~ger, ln the ~ir agitated slurry, dry coating welghts ra~gin~; from 4~5 to . , .: ` .
-10- `

. . ~ F

' `: , :
. . .
.~ , .: :
. . .

~C~55318 135 g/sq. metre. The plates were racked while stîll wet.
Uncoated end plates were used; the brazing alloy of the ~lurry on the exterior heat excharge plates provide~ the - ~iller metal for brazing the end plates. After assel~bly, the unit was dried at 200C for 5 minutes, then placed i~
a furnace filled with dr~ nitro6en. The unit was heated to a temperature of 590C over a 12-mirute period a~d allowed to cool to 550C before removal from the furnace. After cooling to room temperature, the parts were pressure tested ~0 using compressed air at 20 psig. No leaks were detected with those units with a solids coating weight of about 70 g/s~.
- metre or more.
. - .
, ' - ` ' ',' .' - :
~ . ' . ' ' ' ~

, , ' ' ' .. ' ' '~

" , '- .

`

Claims (5)

THE EMBODIMENTS OF THE INVENTION IN WHICH AN EXCLUSIVE
PROPERTY OR PRIVILEGE IS CLAIMED ARE DEFINED AS FOLLOWS:
1. A method of joining aluminium components by means of an aluminium brazing alloy having a melting point lower than that of the aluminium components, in which the assembled components are heated to a temperature above the melting point of the brazing alloy and below the melting point of said components in the presence of a potassium fluoaluminate flux, which is essentially free of un-reacted KF characterised in that the flux and the brazing alloy is applied to the surface of at least one of the components as an aqueous slurry of finely divided flux and metal powder, the film of slurry is then dried and the compon-ents are brazed (after assembly, if necessary) by heating in a dry, oxygen-free inert gas atmosphere, the application of flux/brazing alloy slurry being con-trolled to apply 30-180 gms/m2 of solids and the flux:brazing alloy ratio being selected to deposit at least 3.29 gms/m2 of flux.
2. A method according to claim 1 further characterized in that the ratio of brazing alloy powder to flux in said slurry is in the range of 4-40:1.
3. A method according to claim 1 or 2 further characterized in that the brazing alloy/flux mix is deposited by immersing said one component into a bath of said slurry.
4. A method according to claim 1 or 2 further characterised in that the assembled components are dipped into a bath of said slurry to deposit the brazing alloy/flux mix between the faying surfaces of said assembled components.
5. A method according to any of claims 1 or 2 further characterised in that the inert gas is nitrogen.
CA249,854A 1975-04-09 1976-04-08 Brazing aluminium Expired CA1055318A (en)